MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Nurel Engineering Polymers Promyde® B20 P PA 6, Dry, Heat stabilized, Nucleated and Lubricated
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Heat Stabilized; Nylon 6, Nucleated

Material Notes: Characteristics: Promyde B20 P is a polyamide 6 heat stabilized, lubricated and nucleated for fast cycle and technical injection molding. Its main characteristics are easy flowing, easy mould filling and very fast cooling time whilst maintaining excellent polyamide 6 mechanical properties.

Applications: Due to its easy flow characteristics and very fast cooling time; Promyde B20 P provides significant productivity improvement. Promyde B20 P mould filling is 35 % faster than standard viscosity polyamide 6; that combined with its excellent mechanical and thermal properties make it suitable for high speed multi cavity injection molding for parts such as components used in automotive, electrical, electronics, curtain systems, and also for large technical parts produced in single cavity moulds.

Information provided by Nurel Engineering Polymers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.13 g/cc0.0408 lb/in³ISO 1183
Moisture Absorption 3.00 %3.00 %50%, rh; ISO 62
Water Absorption at Saturation 9.5 %9.5 %in water; ISO 62
Viscosity Test 125 cm³/g1.25 dl/gViscosity Number; ISO 307
Linear Mold Shrinkage, Flow 0.0090 - 0.011 cm/cm0.0090 - 0.011 in/in
Linear Mold Shrinkage, Transverse 0.0080 - 0.011 cm/cm0.0080 - 0.011 in/in
Melt Flow 226 g/10 min
@Load 5.00 kg,
Temperature 275 °C
226 g/10 min
@Load 11.0 lb,
Temperature 527 °F
[cm3/10 min], MVR; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 85.0 MPa12300 psi50 mm/min; ISO 527-1/-2
Elongation at Break 18 %18 %50 mm/min; ISO 527-1/-2
Elongation at Yield 3.5 %3.5 %50 mm/min; ISO 527-1/-2
Tensile Modulus 3.30 GPa479 ksi1 mm/min; ISO 527-1/-2
Flexural Strength 110 MPa16000 psi2 mm/min; ISO 178
Flexural Modulus 2.80 GPa406 ksi2 mm/min; ISO 178
Charpy Impact Unnotched  32.0 J/cm²
@Temperature -30.0 °C
152 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.450 J/cm²
@Temperature -30.0 °C
2.14 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC 60093
Dielectric Constant 3.5
@Frequency 1e+6 Hz
3.5
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 7.00 µm/m-°C
@Temperature 23.0 - 80.0 °C
3.89 µin/in-°F
@Temperature 73.4 - 176 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 100 µm/m-°C
@Temperature 23.0 - 80.0 °C
55.6 µin/in-°F
@Temperature 73.4 - 176 °F
ISO 11359-1/-2
Melting Point 222 °C432 °FDSC 10°C/min; ISO 3146
Deflection Temperature at 0.46 MPa (66 psi) 187 °C369 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °C149 °FISO 75-1/-2
Flammability, UL94 V-2
@Thickness 1.50 mm
V-2
@Thickness 0.0591 in
Glow Wire Ignition Temperature 700 °C
@Thickness 1.50 mm
1290 °F
@Thickness 0.0591 in
IEC 60695-2-12,13
Glow Wire Flammability Index 850 °C
@Thickness 1.50 mm
1560 °F
@Thickness 0.0591 in
IEC 60695-2-12,13
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 - 270 °C482 - 518 °Finjection molding
Mold Temperature 40.0 - 80.0 °C104 - 176 °F
Drying Temperature <= 80.0 °C<= 176 °F
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Nurel Engineering Polymers Promyde® B20 P PA 6, Conditioned, Heat stabilized, Nucleated and Lubricated
Overview of materials for 5000 Series Aluminum Alloy
Overview of materials for Epoxy/Carbon Fiber Composite
Ineos ABS Triax® KU2-3154 ABS + Nylon 6
ExxonMobil Exxtral™ BMV 201 Performance Polyolefin

PNUREL001 / 183366

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.