Celanese Zytel® ST811HS BK038 PA6-HI
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, Impact Grade
Material Notes:
Super Toughened, Heat Stabilized, Polyamide 6
Former DuPont product acquired by Celanese in 2022.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.05
g/cc
0.0379
lb/in³
DAM; ISO 1183
Moisture Absorption
2.30 %
@Thickness 2.00 mm
2.30 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Linear Mold Shrinkage, Flow
0.0090
cm/cm
0.0090
in/in
DAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse
0.014
cm/cm
0.014
in/in
DAM; ISO 294-4, 2577
Mechanical Properties
Metric
English
Comments
Tensile Strength, Yield
31.0
MPa
4500
psi
DAM; ISO 527-1/-2
Elongation at Yield
29 %
29 %
DAM; ISO 527-1/-2
Tensile Modulus
0.400
GPa
58.0
ksi
50% RH; ISO 527-1/-2
0.900
GPa
131
ksi
DAM; ISO 527-1/-2
Flexural Modulus
0.850
GPa
123
ksi
DAM; ISO 178
Poissons Ratio
0.45
0.45
DAM
0.47
0.47
50% RH
Izod Impact, Notched (ISO)
13.0
kJ/m²
@Temperature -40.0 °C
6.19
ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 180/1A
65.0
kJ/m²
@Temperature 23.0 °C
30.9
ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
Izod Impact, Unnotched (ISO)
NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
DAM; ISO 180/1U
Charpy Impact Unnotched
NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
DAM; ISO 179/1eU
Charpy Impact, Notched
1.20
J/cm²
@Temperature -40.0 °C
5.71
ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 179/1eA
8.00
J/cm²
@Temperature 23.0 °C
38.1
ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
130
µm/m-°C
72.2
µin/in-°F
DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow
140
µm/m-°C
77.8
µin/in-°F
DAM; ISO 11359-1/-2
Melting Point
218
°C
424
°F
10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi)
40.0
°C
104
°F
DAM; ISO 75-1/-2
Glass Transition Temp, Tg
0.000
°C
32.0
°F
10°C/min; 50% RH; ISO 11357-1/-2
50.0
°C
122
°F
10°C/min; DAM; ISO 11357-1/-2
Flame Spread
<=
80.0
mm/min
@Thickness 1.00 mm
<=
3.15
in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
Processing Properties
Metric
English
Comments
Melt Temperature
240
°C
464
°F
Optimum, Extrusion
235
-
250
°C
455
-
482
°F
Range, Extrusion
260
-
280
°C
500
-
536
°F
Range, Injection
270
°C
518
°F
Optimum, Injection
Mold Temperature
70.0
°C
158
°F
Optimum, Injection
50.0
-
90.0
°C
122
-
194
°F
Injection
Ejection Temperature
190
°C
374
°F
Injection
Drying Temperature
60.0
°C
140
°F
Injection
60.0
°C
140
°F
Extrusion
Dry Time
2.00
-
4.00
hour
2.00
-
4.00
hour
Injection, Dehumidified Dryer
4.00
-
6.00
hour
4.00
-
6.00
hour
Extrusion, Dehumidified Dryer
Moisture Content
<= 0.060 %
<= 0.060 %
Extrusion
<= 0.20 %
<= 0.20 %
Injection
Hold Pressure
50.0
-
100
MPa
7250
-
14500
psi
Range, Injection
Descriptive Properties
Drying Recommended
yes
Injection
FMVSS Class
B
ISO 3795 (FMVSS 302)
ISO designation
ISO 16396-PA6-I,,M1CG1HR,S14-010
Max. screw tangential speed (m/s)
0.3
Injection
Part Marking Code
>PA6-HI<
ISO 11469
Polymer
PA6-I
Processing Hold Pressure Time (s/mm)
4
Injection
Regional Availability
Asia Pacific
Europe
Near East/Africa
North America
South and Central America
Resin Identification
PA6-HI
ISO 1043
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Celanese Zytel® ST811HS NC010 PA6-HI
Toyobo PELPRENE™ S3002 Polyester TPE, Ultra Heat-resistant
Celanese Zytel® ST7301 BK356 PA6-HI
Celanese Zytel® ST7301 NC010 PA6-HI
Celanese Zytel® ST801AHS NC010 PA66-HI
PDSX5515 / 198155
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.