MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Barlog Plastics KEBATER PBT A9030 gray 037091 (DB) PBT+PET, 30% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); PBT + PET Blend, Glass Filled

Material Notes: PBT+PET, 30% glass fiber reinforced grey, suitable for contact with food (EU)

Properties: dimensionally stable, good chemical resistance, good gliding properties, High strength, High stiffness, High wear resistance, semi-crystalline, approved for food contact (EU and FDA)

Typical areas of application: Cover, Electronic components, Housing, Crockery and cutlery, Food packaging, Connecting elements

Industries: Automotive, Electrical and electronics industry, Household appliances, Food processing industry, Mechanical Engineering, Sanitary industry

Information provided by BARLOG plastics GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.53 g/ccISO 1183-1
Melt Flow 20.0 g/10 min
@Load 2.16 kg,
Temperature 270 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 120 MPaISO 527-1
Elongation at Break 2.00 %ISO 527-1
Modulus of Elasticity 8.50 GPaISO 527-1
Charpy Impact Unnotched 35.0 kJ/m²ISO 179-1eU
 
Thermal PropertiesOriginal ValueComments
Flammability, UL94 HB
@Thickness 0.400 mm
IEC 60695-11-10
 HB
@Thickness 0.800 mm
IEC 60695-11-10
 HB
@Thickness 1.60 mm
IEC 60695-11-10
 HB
@Thickness 3.20 mm
IEC 60695-11-10
 
Processing PropertiesOriginal ValueComments
Melt Temperature 255 - 275 °C
Mold Temperature 80.0 - 120 °C
Drying Temperature 100 - 120 °C
Dry Time 2.00 - 4.00 hour
Moisture Content <= 0.0200 %
Back Pressure <= 4.00 MPa
 
Compliance PropertiesOriginal ValueComments
FDA Yes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBARLO689 / 326763

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.