Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 4.71 g/cc | 4.71 g/cc |
|
Chemical Properties | Metric | English | Comments |
---|
Acid Class, SR | 51.2 | 51.2 |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 520 @Load 0.0999 kg | 520 @Load 0.220 lb |
Modulus of Elasticity | 95.3 GPa | 13800 ksi |
Modulus of Rigidity | 36.6 GPa | 5310 ksi |
Poissons Ratio | 0.302 | 0.302 |
Abrasion | 160 | 160 |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 8.50 µm/m-°C @Temperature -30.0 - 70.0 °C | 4.72 µin/in-°F @Temperature -22.0 - 158 °F |
| 9.80 µm/m-°C @Temperature 100 - 300 °C | 5.44 µin/in-°F @Temperature 212 - 572 °F |
Thermal Conductivity | 0.701 W/m-K @Temperature 35.0 °C | 4.86 BTU-in/hr-ft²-°F @Temperature 95.0 °F |
Transformation Temperature, Tg | 655 °C | 1210 °F |
Softening Point | 721 °C | 1330 °F |
Annealing Point | 635 °C | 1180 °F |
Strain Point | 609 °C | 1130 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.7881 @Wavelength 2325.42 nm | 1.7881 @Wavelength 2325.42 nm |
| 1.7943 @Wavelength 1970.09 nm | 1.7943 @Wavelength 1970.09 nm |
| 1.80135 @Wavelength 1529.58 nm | 1.80135 @Wavelength 1529.58 nm |
| 1.80854 @Wavelength 1128.64 nm | 1.80854 @Wavelength 1128.64 nm |
| 1.81125 @Wavelength 1013.98 nm | 1.81125 @Wavelength 1013.98 nm |
| 1.81641 @Wavelength 852.11 nm | 1.81641 @Wavelength 852.11 nm |
| 1.82017 @Wavelength 768.19 nm | 1.82017 @Wavelength 768.19 nm |
| 1.82374 @Wavelength 706.52 nm | 1.82374 @Wavelength 706.52 nm |
| 1.82739 @Wavelength 656.27 nm | 1.82739 @Wavelength 656.27 nm |
| 1.82843 @Wavelength 643.85 nm | 1.82843 @Wavelength 643.85 nm |
| 1.8294 @Wavelength 632.8 nm | 1.8294 @Wavelength 632.8 nm |
| 1.8338 @Wavelength 589.29 nm | 1.8338 @Wavelength 589.29 nm |
| 1.834 @Wavelength 587.56 nm | 1.834 @Wavelength 587.56 nm |
| 1.83932 @Wavelength 546.07 nm | 1.83932 @Wavelength 546.07 nm |
| 1.84983 @Wavelength 486.13 nm | 1.84983 @Wavelength 486.13 nm |
| 1.85116 @Wavelength 479.99 nm | 1.85116 @Wavelength 479.99 nm |
| 1.86106 @Wavelength 441.57 nm | 1.86106 @Wavelength 441.57 nm |
| 1.86281 @Wavelength 435.835 nm | 1.86281 @Wavelength 435.835 nm |
| 1.87401 @Wavelength 404.656 nm | 1.87401 @Wavelength 404.656 nm |
| 1.89407 @Wavelength 365.015 nm | 1.89407 @Wavelength 365.015 nm |
Abbe Number | 36.92 | 36.92 |
| 37.17 | 37.17 |
Optical Dispersion | 0.006608 | 0.006608 |
| 0.007222 | 0.007222 |
| 0.010892 | 0.010892 |
| 0.011196 | 0.011196 |
| 0.011843 | 0.011843 |
| 0.011929 | 0.011929 |
| 0.012981 | 0.012981 |
| 0.016137 | 0.016137 |
| 0.017174 | 0.017174 |
| 0.022437 | 0.022437 |
| 0.022735 | 0.022735 |
| 0.02881 | 0.02881 |
| 0.031262 | 0.031262 |
| 0.042908 | 0.042908 |
Transmission, Visible | 83 % @Thickness 10.0 mm, Wavelength 380 nm | 83 % @Thickness 0.394 in, Wavelength 380 nm |
| 89 % @Thickness 10.0 mm, Wavelength 390 nm | 89 % @Thickness 0.394 in, Wavelength 390 nm |
| 92.7 % @Thickness 10.0 mm, Wavelength 400 nm | 92.7 % @Thickness 0.394 in, Wavelength 400 nm |
| 95.7 % @Thickness 10.0 mm, Wavelength 420 nm | 95.7 % @Thickness 0.394 in, Wavelength 420 nm |
| 96.8 % @Thickness 10.0 mm, Wavelength 440 nm | 96.8 % @Thickness 0.394 in, Wavelength 440 nm |
| 97.6 % @Thickness 10.0 mm, Wavelength 460 nm | 97.6 % @Thickness 0.394 in, Wavelength 460 nm |
| 98.3 % @Thickness 10.0 mm, Wavelength 480 nm | 98.3 % @Thickness 0.394 in, Wavelength 480 nm |
| 98.9 % @Thickness 10.0 mm, Wavelength 500 nm | 98.9 % @Thickness 0.394 in, Wavelength 500 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 550 nm | 99.5 % @Thickness 0.394 in, Wavelength 550 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 600 nm | 99.5 % @Thickness 0.394 in, Wavelength 600 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 650 nm | 99.5 % @Thickness 0.394 in, Wavelength 650 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 700 nm | 99.7 % @Thickness 0.394 in, Wavelength 700 nm |
IR Transmittance | 80 % @Thickness 10.0 mm, Wavelength 2400 nm | 80 % @Thickness 0.394 in, Wavelength 2400 nm |
| 92.7 % @Thickness 10.0 mm, Wavelength 2200 nm | 92.7 % @Thickness 0.394 in, Wavelength 2200 nm |
| 96.8 % @Thickness 10.0 mm, Wavelength 2000 nm | 96.8 % @Thickness 0.394 in, Wavelength 2000 nm |
| 98.6 % @Thickness 10.0 mm, Wavelength 1800 nm | 98.6 % @Thickness 0.394 in, Wavelength 1800 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 1600 nm | 99.5 % @Thickness 0.394 in, Wavelength 1600 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 800 nm | 99.8 % @Thickness 0.394 in, Wavelength 800 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 900 nm | 99.8 % @Thickness 0.394 in, Wavelength 900 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 1000 nm | 99.8 % @Thickness 0.394 in, Wavelength 1000 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 1400 nm | 99.8 % @Thickness 0.394 in, Wavelength 1400 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 1200 nm | 99.9 % @Thickness 0.394 in, Wavelength 1200 nm |
UV Transmittance | 8.0 % @Thickness 10.0 mm, Wavelength 340 nm | 8.0 % @Thickness 0.394 in, Wavelength 340 nm |
| 31 % @Thickness 10.0 mm, Wavelength 350 nm | 31 % @Thickness 0.394 in, Wavelength 350 nm |
| 56 % @Thickness 10.0 mm, Wavelength 360 nm | 56 % @Thickness 0.394 in, Wavelength 360 nm |
| 73 % @Thickness 10.0 mm, Wavelength 370 nm | 73 % @Thickness 0.394 in, Wavelength 370 nm |
|
Descriptive Properties |
---|
Acid Resistance, Powder Method, RA(P) | 3 |
CCI | 0.00 B |
| 1.58 G |
| 1.58 R |
coloring, λ 5 | 340 |
coloring, λ 80 | 425 |
Coloring, Internal Transmission λ 0.05 | 336 |
Coloring, Internal Transmission λ 0.80 | 377 |
Knoop Hardness Class | 5 |
Ohara Code d | 834372 |
Ohara Code e | 839369 |
Phosphate Resistance, PR | 1.2 |
Photoelastic Constant (ß) | 1.36 |
Water Resistance, RW(P) | 1 |
Weathering Resistance (Surface Method) W(S)max | 3 |
Yield Point, At (°C) | 688 |