Physical Properties | Original Value | Comments |
---|
Density | 4.22 g/cc |
|
Chemical Properties | Original Value | Comments |
---|
Acid Class, SR | 51.3 |
Alkali Class, AR | 1.0 |
Stain Resistance Class, FR | 1.0 |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Knoop | 797 |
Modulus of Elasticity | 122 GPa |
Poissons Ratio | 0.295 |
Shear Modulus | 47.1 GPa |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 5.80 µm/m-°C @Temperature -30.0 - 70.0 °C |
| 7.10 µm/m-°C @Temperature 20.0 - 300 °C |
Specific Heat Capacity | 0.560 J/g-°C |
Thermal Conductivity | 0.890 W/m-K |
Transformation Temperature, Tg | 668 °C |
Softening Point | 750 °C |
Annealing Point | 670 °C |
|
Optical Properties | Original Value | Comments |
---|
Refractive Index | 1.713 @Wavelength 2323.4 nm |
| 1.721 @Wavelength 1970.1 nm |
| 1.729 @Wavelength 1529.6 nm |
| 1.737 @Wavelength 1060 nm |
| 1.738 @Wavelength 1014 nm |
| 1.74292 @Wavelength 852.1 nm |
| 1.748 @Wavelength 706.5 nm |
| 1.75 @Wavelength 656.3 nm |
| 1.751 @Wavelength 632.8 nm |
| 1.751 @Wavelength 643.8 nm |
| 1.754 @Wavelength 589.3 nm |
| 1.755 @Wavelength 587.6 nm |
| 1.758 @Wavelength 546.1 nm |
| 1.765 @Wavelength 480 nm |
| 1.765 @Wavelength 486.1 nm |
| 1.772 @Wavelength 435.8 nm |
| 1.779 @Wavelength 404.7 nm |
| 1.79 @Wavelength 365 nm |
| 1.803 @Wavelength 334.1 nm |
| 1.814 @Wavelength 312.6 nm |
| 1.824 @Wavelength 296.7 nm |
Abbe Number | 52.07 |
| 52.3 |
Optical Dispersion | 0.014436 |
| 0.014566 |
Transmission, Visible | 97.1 % @Thickness 25.0 mm, Wavelength 420 nm |
| 97.9 % @Thickness 25.0 mm, Wavelength 436 nm |
| 98.6 % @Thickness 25.0 mm, Wavelength 460 nm |
| 98.8 % @Thickness 10.0 mm, Wavelength 420 nm |
| 99.2 % @Thickness 10.0 mm, Wavelength 436 nm |
| 99.3 % @Thickness 25.0 mm, Wavelength 620 nm |
| 99.3 % @Thickness 25.0 mm, Wavelength 500 nm |
| 99.4 % @Thickness 25.0 mm, Wavelength 660 nm |
| 99.4 % @Thickness 25.0 mm, Wavelength 580 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 460 nm |
| 99.5 % @Thickness 25.0 mm, Wavelength 700 nm |
| 99.5 % @Thickness 25.0 mm, Wavelength 546 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 500 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 620 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 546 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 700 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 660 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 580 nm |
IR Transmittance | 10 % @Thickness 25.0 mm, Wavelength 2500 nm |
| 38 % @Thickness 25.0 mm, Wavelength 2325 nm |
| 39.8 % @Thickness 10.0 mm, Wavelength 2500 nm |
| 67.9 % @Thickness 10.0 mm, Wavelength 2325 nm |
| 85 % @Thickness 25.0 mm, Wavelength 1970 nm |
| 93.7 % @Thickness 10.0 mm, Wavelength 1970 nm |
| 96.3 % @Thickness 25.0 mm, Wavelength 1530 nm |
| 98.5 % @Thickness 10.0 mm, Wavelength 1530 nm |
| 99.5 % @Thickness 25.0 mm, Wavelength 1060 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 1060 nm |
UV Transmittance | 1.0 % @Thickness 25.0 mm, Wavelength 300 nm |
| 2.2 % @Thickness 10.0 mm, Wavelength 280 nm |
| 3.0 % @Thickness 25.0 mm, Wavelength 310 nm |
| 11.8 % @Thickness 10.0 mm, Wavelength 290 nm |
| 14 % @Thickness 25.0 mm, Wavelength 320 nm |
| 21.7 % @Thickness 10.0 mm, Wavelength 300 nm |
| 28.3 % @Thickness 10.0 mm, Wavelength 310 nm |
| 35 % @Thickness 25.0 mm, Wavelength 334 nm |
| 45.5 % @Thickness 10.0 mm, Wavelength 320 nm |
| 61 % @Thickness 25.0 mm, Wavelength 350 nm |
| 65.7 % @Thickness 10.0 mm, Wavelength 334 nm |
| 79 % @Thickness 25.0 mm, Wavelength 365 nm |
| 82.1 % @Thickness 10.0 mm, Wavelength 350 nm |
| 83 % @Thickness 25.0 mm, Wavelength 370 nm |
| 89 % @Thickness 25.0 mm, Wavelength 380 nm |
| 91 % @Thickness 10.0 mm, Wavelength 365 nm |
| 92.8 % @Thickness 10.0 mm, Wavelength 370 nm |
| 93 % @Thickness 25.0 mm, Wavelength 390 nm |
| 95 % @Thickness 25.0 mm, Wavelength 400 nm |
| 95.4 % @Thickness 10.0 mm, Wavelength 380 nm |
| 95.6 % @Thickness 25.0 mm, Wavelength 405 nm |
| 97.1 % @Thickness 10.0 mm, Wavelength 390 nm |
| 98 % @Thickness 10.0 mm, Wavelength 400 nm |
| 98.2 % @Thickness 10.0 mm, Wavelength 405 nm |
|
Descriptive Properties |
---|
Acid resistance class | 4 |
Climatic resistance | 1 |
Phosphate resistance | 2 |
Stress optical coefficient | 1.43 |
Water resistance class | 1 |
Yield point/sag temperature | 702°C |