MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sandvik 2R68/2R68HV Seamless tube and pipe
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Sandvik 2R68 is a molybdenum alloyed austenitic chromium-nickel steel. It is characterized by low contents of manganese, sulphur, carbon and nitrogen. This results in a very clean steel with a low content of non-metallic inclusions. The grade is especially developed for a application where very high demands are set upon allowed limits of contamination from the stainless steel material. Typical examples are applications found within the semiconductor and pharmaceutical industries.

The steel is available in two forms: Sandvik 2R68, produced by conventional AOD technique, and Sandvik 2R68HV, further optimized by vacuum arc remelting (VAR) of the AOD material. The VAR treatment reduces the content of oxide inclusions, thereby obtaining further cleanliness. Otherwise the two grades generally have similar properties.

Electropolishing of the grade produces very even and smooth surfaces, thanks to the very low levels of impurities. The tubes are used in the electropolished condition for high purity gas distribution systems.

Information provided by Sandvik

ASTM 316L; EN 1.4435

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.00 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 155
Tensile Strength, Ultimate 490 - 690 MPa
Tensile Strength, Yield >= 190 MPa
@Strain 0.2 %
 >= 225 MPa
@Strain 1 %
 >= 100 MPa
@Strain 0.2 %,
Temperature 500 °C
 >= 118 MPa
@Strain 0.2 %,
Temperature 300 °C
 >= 128 MPa
@Strain 1 %,
Temperature 500 °C
 >= 145 MPa
@Strain 1 %,
Temperature 300 °C
Elongation at Break >= 40 %
 >= 35 %
@Thickness 50.8 mm
Modulus of Elasticity 200 GPa
 165 GPa
@Temperature 500 °C
 179 GPa
@Temperature 300 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.0 µm/m-°C
@Temperature 30.0 - 100 °C
 17.0 µm/m-°C
@Temperature 30.0 - 200 °C
 21.0 µm/m-°C
@Temperature 30.0 - 500 °C
Specific Heat Capacity 0.485 J/g-°C
@Temperature 20.0 °C
 0.515 J/g-°C
@Temperature 200 °C
 0.540 J/g-°C
@Temperature 400 °C
 0.575 J/g-°C
@Temperature 600 °C
Thermal Conductivity 14.0 W/m-K
@Temperature 20.0 °C
 17.0 W/m-K
@Temperature 200 °C
 20.0 W/m-K
@Temperature 400 °C
 23.0 W/m-K
@Temperature 600 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.020 %
Chromium, Cr 17.5 %
Iron, Fe 63.9 %As Balance
Manganese, Mn <= 0.40 %
Molybdenum, Mo 2.6 %
Nickel, Ni 14.5 %
Phosphorus, P <= 0.030 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.0030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Sandvik 2RK65 Seamless tube and pipe
Industeel CLC 1.2312 Prehardened Mold Steel (300HB/32HRC) with Improved Machinability
Industeel CLC 1.2311 Prehardened Mold Steel (300HB/30HRC)
Carpenter BioDur™ 316LS Stainless Medical Implant Alloy, Annealed
Medical Grade Stainless Steel 316LVM

NSANDV227 / 19121

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.