MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Sandvik 2RK65 Seamless tube and pipe
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Sandvik 2RK65 is an austenitic stainless ELC steel intended for use under severe corrosion conditions within the process industry. The material is characterized by the following properties:
  • very good resistance to attacks in acidic environments, e.g. sulphuric, phosphoric and acetic acid
  • very good resistance to pitting in neutral chloride-bearing solutions
  • much better resistance to crevice corrosion than steels of the AISI 304 and AISI 316 type
  • very good resistance to stress corrosion cracking
  • good weldability
  • Information provided by Sandvik

    UNS N08904; EN 1.4539

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 8.00 g/cc0.289 lb/in³
     
    Mechanical PropertiesMetricEnglishComments
    Hardness, Vickers 160160
    Tensile Strength, Ultimate 520 - 720 MPa75400 - 104000 psi
    Tensile Strength, Yield  >= 230 MPa
    @Strain 0.2 %
    >= 33400 psi
    @Strain 0.2 %
     >= 250 MPa
    @Strain 1 %
    >= 36300 psi
    @Strain 1 %
     >= 125 MPa
    @Strain 0.2 %,
    Temperature 400 °C
    >= 18100 psi
    @Strain 0.2 %,
    Temperature 752 °F
     >= 125 MPa
    @Strain 0.2 %,
    Temperature 400 °C
    >= 18100 psi
    @Strain 0.2 %,
    Temperature 752 °F
     >= 136 MPa
    @Strain 1 %,
    Temperature 300 °C
    >= 19700 psi
    @Strain 1 %,
    Temperature 572 °F
     >= 155 MPa
    @Strain 0.2 %,
    Temperature 200 °C
    >= 22500 psi
    @Strain 0.2 %,
    Temperature 392 °F
     >= 155 MPa
    @Strain 1 %,
    Temperature 400 °C
    >= 22500 psi
    @Strain 1 %,
    Temperature 752 °F
     >= 155 MPa
    @Strain 1 %,
    Temperature 400 °C
    >= 22500 psi
    @Strain 1 %,
    Temperature 752 °F
     >= 155 MPa
    @Strain 0.2 %,
    Temperature 200 °C
    >= 22500 psi
    @Strain 0.2 %,
    Temperature 392 °F
     >= 165 MPa
    @Strain 1 %,
    Temperature 300 °C
    >= 23900 psi
    @Strain 1 %,
    Temperature 572 °F
     >= 176 MPa
    @Strain 0.2 %,
    Temperature 100 °C
    >= 25500 psi
    @Strain 0.2 %,
    Temperature 212 °F
     >= 185 MPa
    @Strain 1 %,
    Temperature 200 °C
    >= 26800 psi
    @Strain 1 %,
    Temperature 392 °F
     >= 185 MPa
    @Strain 1 %,
    Temperature 200 °C
    >= 26800 psi
    @Strain 1 %,
    Temperature 392 °F
     >= 205 MPa
    @Strain 0.2 %,
    Temperature 100 °C
    >= 29700 psi
    @Strain 0.2 %,
    Temperature 212 °F
    Elongation at Break >= 35 %>= 35 %
     >= 35 %
    @Thickness 50.8 mm
    >= 35 %
    @Thickness 2.00 in
    Modulus of Elasticity 195 GPa28300 ksi
     158 GPa
    @Temperature 500 °C
    22900 ksi
    @Temperature 932 °F
     166 GPa
    @Temperature 400 °C
    24100 ksi
    @Temperature 752 °F
     174 GPa
    @Temperature 300 °C
    25200 ksi
    @Temperature 572 °F
     182 GPa
    @Temperature 200 °C
    26400 ksi
    @Temperature 392 °F
     190 GPa
    @Temperature 100 °C
    27600 ksi
    @Temperature 212 °F
     
    Electrical PropertiesMetricEnglishComments
    Electrical Resistivity  0.0000940 ohm-cm
    @Temperature 20.0 °C
    0.0000940 ohm-cm
    @Temperature 68.0 °F
     0.0000990 ohm-cm
    @Temperature 100 °C
    0.0000990 ohm-cm
    @Temperature 212 °F
     0.000107 ohm-cm
    @Temperature 200 °C
    0.000107 ohm-cm
    @Temperature 392 °F
     0.000113 ohm-cm
    @Temperature 300 °C
    0.000113 ohm-cm
    @Temperature 572 °F
     0.000114 ohm-cm
    @Temperature 500 °C
    0.000114 ohm-cm
    @Temperature 932 °F
     0.000115 ohm-cm
    @Temperature 600 °C
    0.000115 ohm-cm
    @Temperature 1110 °F
     0.000115 ohm-cm
    @Temperature 400 °C
    0.000115 ohm-cm
    @Temperature 752 °F
     0.000118 ohm-cm
    @Temperature 700 °C
    0.000118 ohm-cm
    @Temperature 1290 °F
     
    Thermal PropertiesMetricEnglishComments
    CTE, linear  15.5 µm/m-°C
    @Temperature 30.0 - 100 °C
    8.61 µin/in-°F
    @Temperature 86.0 - 212 °F
     16.0 µm/m-°C
    @Temperature 30.0 - 200 °C
    8.89 µin/in-°F
    @Temperature 86.0 - 392 °F
     16.0 µm/m-°C
    @Temperature 30.0 - 200 °C
    8.89 µin/in-°F
    @Temperature 86.0 - 392 °F
     16.5 µm/m-°C
    @Temperature 300 °C
    9.17 µin/in-°F
    @Temperature 572 °F
     17.0 µm/m-°C
    @Temperature 400 °C
    9.44 µin/in-°F
    @Temperature 752 °F
     17.0 µm/m-°C
    @Temperature 30.0 - 500 °C
    9.44 µin/in-°F
    @Temperature 86.0 - 932 °F
     17.0 µm/m-°C
    @Temperature 30.0 - 400 °C
    9.44 µin/in-°F
    @Temperature 86.0 - 752 °F
     17.5 µm/m-°C
    @Temperature 30.0 - 600 °C
    9.72 µin/in-°F
    @Temperature 86.0 - 1110 °F
     17.5 µm/m-°C
    @Temperature 600 °C
    9.72 µin/in-°F
    @Temperature 1110 °F
     17.5 µm/m-°C
    @Temperature 30.0 - 700 °C
    9.72 µin/in-°F
    @Temperature 86.0 - 1290 °F
    Specific Heat Capacity  0.460 J/g-°C
    @Temperature 20.0 °C
    0.110 BTU/lb-°F
    @Temperature 68.0 °F
     0.485 J/g-°C
    @Temperature 100 °C
    0.116 BTU/lb-°F
    @Temperature 212 °F
     0.485 J/g-°C
    @Temperature 100 °C
    0.116 BTU/lb-°F
    @Temperature 212 °F
     0.515 J/g-°C
    @Temperature 200 °C
    0.123 BTU/lb-°F
    @Temperature 392 °F
     0.545 J/g-°C
    @Temperature 300 °C
    0.130 BTU/lb-°F
    @Temperature 572 °F
     0.545 J/g-°C
    @Temperature 300 °C
    0.130 BTU/lb-°F
    @Temperature 572 °F
     0.570 J/g-°C
    @Temperature 400 °C
    0.136 BTU/lb-°F
    @Temperature 752 °F
     0.590 J/g-°C
    @Temperature 500 °C
    0.141 BTU/lb-°F
    @Temperature 932 °F
     0.590 J/g-°C
    @Temperature 500 °C
    0.141 BTU/lb-°F
    @Temperature 932 °F
     0.605 J/g-°C
    @Temperature 600 °C
    0.145 BTU/lb-°F
    @Temperature 1110 °F
     0.615 J/g-°C
    @Temperature 700 °C
    0.147 BTU/lb-°F
    @Temperature 1290 °F
     0.615 J/g-°C
    @Temperature 700 °C
    0.147 BTU/lb-°F
    @Temperature 1290 °F
    Thermal Conductivity  12.0 W/m-K
    @Temperature 20.0 °C
    83.3 BTU-in/hr-ft²-°F
    @Temperature 68.0 °F
     14.0 W/m-K
    @Temperature 100 °C
    97.2 BTU-in/hr-ft²-°F
    @Temperature 212 °F
     14.0 W/m-K
    @Temperature 100 °C
    97.2 BTU-in/hr-ft²-°F
    @Temperature 212 °F
     16.0 W/m-K
    @Temperature 200 °C
    111 BTU-in/hr-ft²-°F
    @Temperature 392 °F
     18.0 W/m-K
    @Temperature 300 °C
    125 BTU-in/hr-ft²-°F
    @Temperature 572 °F
     18.0 W/m-K
    @Temperature 300 °C
    125 BTU-in/hr-ft²-°F
    @Temperature 572 °F
     20.0 W/m-K
    @Temperature 400 °C
    139 BTU-in/hr-ft²-°F
    @Temperature 752 °F
     22.0 W/m-K
    @Temperature 500 °C
    153 BTU-in/hr-ft²-°F
    @Temperature 932 °F
     22.0 W/m-K
    @Temperature 500 °C
    153 BTU-in/hr-ft²-°F
    @Temperature 932 °F
     23.0 W/m-K
    @Temperature 600 °C
    160 BTU-in/hr-ft²-°F
    @Temperature 1110 °F
     25.0 W/m-K
    @Temperature 700 °C
    174 BTU-in/hr-ft²-°F
    @Temperature 1290 °F
     25.0 W/m-K
    @Temperature 700 °C
    174 BTU-in/hr-ft²-°F
    @Temperature 1290 °F
     
    Component Elements PropertiesMetricEnglishComments
    Carbon, C <= 0.020 %<= 0.020 %
    Chromium, Cr 20 %20 %
    Copper, Cu 1.5 %1.5 %
    Iron, Fe 46.6 %46.6 %As Balance
    Manganese, Mn 1.8 %1.8 %
    Molybdenum, Mo 4.5 %4.5 %
    Nickel, Ni 25 %25 %
    Phosphorus, P <= 0.025 %<= 0.025 %
    Silicon, Si 0.50 %0.50 %
    Sulfur, S <= 0.015 %<= 0.015 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    ATI Allegheny Ludlum Stainless Steel Type 439/AL 439HP™ (ASTM XM-8; UNS S43035)
    Eagle Brass 304 Austenitic Stainless Steel, Full Hardened
    Eagle Brass 304 Austenitic Stainless Steel, 3/4 Hardened
    Sandvik 2R68/2R68HV Seamless tube and pipe
    304 Stainless Steel (UNS S30400); 1/2 Hard Bar, Plate, Sheet, and Strip

    NSANDV230 / 19124

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.