MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Trinseo Magnum™ 358HP ABS, High Heat  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Heat Resistant, Molded

Material Notes: MAGNUM® ABS resins are thermoplastic materials which provide an excellent balance of processability, impact resistance and heat resistance as imparted by the various polymer compositions. MAGNUM ABS resin are available in a wide range of melt flow rates, impact strength and heat resistance for both high and low gloss applications manufactured by injection molding, sheet or profile extrusion and thermoforming.

The Automotive grades of MAGNUM ABS resins offer a wide range of gloss, viscosity, impact strength and heat properties for use in numerous automotive applications. Melt flow rates from 1 to 12 g/10 min, impact strengths from 130 to 590 J/m and heat distortion temperatures from 77.C to 90.C are available. Available primarily as natural plus concentrates, MAGNUM ABS resins are used in a wide variety of automotive applications including structural instrument panels, consoles, pillars and exterior trim parts requiring painting and plating.

MAGNUM 358 HP ABS resin is a high heat, low gloss resin having unannealed DTUL values of 90.C at 1.8 MPa loading. MAGNUM 358 HP ABS resin is often used in switch plates, demister grilles and door rollovers, and visor covers.

Data provided by Dow Chemical.

This product line was spun off from Dow Chemical to Styron in 2010.

Key Words: Poly(Acrylonitrile Butadiene Styrene)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.04 g/ccASTM Data
Linear Mold Shrinkage 0.0055 cm/cm
Melt Flow 2.5 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM Data
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 40.0 MPaISO Data
Tensile Strength, Yield 47.6 MPaASTM Data
Elongation at Break 15 %ASTM Data
Tensile Modulus 2.34 GPaASTM Data
Izod Impact, Notched 2.19 J/cmASTM Data
Charpy Impact Unnotched 6.00 J/cm²ISO Data, Low Temp
 NBISO Data
Charpy Impact, Notched 0.700 J/cm²ISO Data, Low Temp
 1.80 J/cm²ISO Data
Instrumented Impact Total Energy 21.0 J
@Temperature -30.0 °C
 42.0 J
@Temperature 23.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 77.4 µm/m-°C
@Temperature 20.0 °C
ASTM data
Deflection Temperature at 0.46 MPa (66 psi) 105 °CUnannealed; ASTM Data
Deflection Temperature at 1.8 MPa (264 psi) 90.0 °CUnannealed; ASTM Data
Vicat Softening Point 117 °C

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Trinseo Magnum™ 344HP ABS
Trinseo Magnum™ 344CC ABS
Trinseo Magnum™ 342EZ ABS, Medium Impact
Trinseo Magnum™ 357HP ABS, High Heat
Trinseo Magnum™ 780HP ABS, High Heat, High Impact

PZZDW089 / 34320

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.