MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Telcar® TELC-1000-105 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic

Material Notes: Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: High Hardness; Low Density; Low Flow; Low Specific Gravity; Without Fillers

Uses: General Purpose; Industrial Applications

Agency Rating: UL 94

RoHS Compliant:RoHS Compliant

UL File Number: QMFZ2.E54709

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.892 g/cc0.0322 lb/in³ASTM D792
Viscosity 378 cP
@Shear Rate 206 1/s,
Temperature 200 °C
378 cP
@Shear Rate 206 1/s,
Temperature 392 °F
ASTM D3835
Melt Flow 4.5 g/10 min
@Load 2.16 kg,
Temperature 230 °C
4.5 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 59
@Time 5.00 sec
59
@Time 0.00139 hour
ASTM D2240
 62.2
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
62.2
@Treatment Temp. 230 °F,
Time 1008 hour
Change in Air
Tensile Strength at Break 13.4 MPa1940 psiAcross Flow; ASTM D412
 15.9 MPa2310 psiFlow; ASTM D412
Tensile Strength  11.2 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
1630 psi
@Treatment Temp. 257 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
 11.4 MPa
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
1650 psi
@Treatment Temp. 230 °F,
Time 1008 hour
Across Flow, Change in Air; ISO 188
Tensile Stress at Strain  11.0 MPa
@Strain 100 %
1600 psi
@Strain 100 %
Across Flow; ASTM D412
 13.1 MPa
@Strain 100 %
1900 psi
@Strain 100 %
Flow; ASTM D412
Elongation at Break 230 %230 %Flow; ASTM D412
 290 %290 %Across Flow; ASTM D412
 191 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
191 %
@Treatment Temp. 230 °F,
Time 1008 hour
Across Flow, Change in Air; ISO 188
 235 %
@Treatment Temp. 125 °C,
Time 605000 sec
235 %
@Treatment Temp. 257 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
Tear Strength 121 kN/m691 pliAcross Flow, Die C; ASTM D624
Compression Set  54 %
@Temperature 22.8 °C,
Time 79200 sec
54 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D695
 74 %
@Temperature 70.0 °C,
Time 79200 sec
74 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D695
 93 %
@Temperature 90.0 °C,
Time 252000 sec
93 %
@Temperature 194 °F,
Time 70.0 hour
ASTM D695
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -55.0 °C-67.0 °FASTM D746
UL RTI, Electrical 50.0 °C122 °FUL 746
UL RTI, Mechanical with Impact 50.0 °C122 °FUL 746
UL RTI, Mechanical without Impact 50.0 °C122 °FUL 746
Flammability, UL94 HB
@Thickness 0.762 mm
HB
@Thickness 0.0300 in
All Colors
 
Processing PropertiesMetricEnglishComments
Processing Temperature 188 - 210 °C370 - 410 °FInjection, Melt
Rear Barrel Temperature 171 - 193 °C340 - 380 °FInjection
Middle Barrel Temperature 177 - 199 °C350 - 390 °FInjection
Front Barrel Temperature 182 - 204 °C360 - 400 °FInjection
Nozzle Temperature 188 - 210 °C370 - 410 °FInjection
Zone 1 166 - 188 °C330 - 370 °FExtrusion
Zone 2 171 - 193 °C340 - 380 °FExtrusion
Zone 3 177 - 199 °C350 - 390 °FExtrusion
Zone 5 182 - 204 °C360 - 400 °FExtrusion
Die Temperature 190 - 210 °C374 - 410 °FExtrusion
Mold Temperature 25.0 - 65.6 °C77.0 - 150 °FInjection
Drying Temperature 80.0 °C176 °F
Dry Time 2.00 hour2.00 hour
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psiInjection
Back Pressure 0.172 - 0.345 MPa25.0 - 50.0 psiInjection
Cushion 0.381 - 2.54 cm0.150 - 1.00 inInjection
Screw Speed 30 - 100 rpm30 - 100 rpmExtrusion
 50 - 100 rpm50 - 100 rpmInjection
 
Descriptive Properties
AppearanceTranslucent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1630 / 238121

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.