System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
AISI Type D2 Tool Steel, air-quenched from 1010°C, tempered at 450°C
Categories:
Metal
;
Ferrous Metal
;
Carbon Steel
;
High Carbon Steel
;
Tool Steel
;
Cold Work Steel
Material Notes:
high carbon, high chromium
Key Words:
UNS T30402, ASTM A681, FED QQ-T-570, SAE J437, SAE J438, DIN 1.2379, B. JIS G4404(83) SKD11 SKD-11 SDK 11
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
7.70
g/cc
Mechanical Properties
Original Value
Comments
Hardness, Knoop
682
Converted from Rockwell C hardness.
Hardness, Rockwell C
58
Hardness, Vickers
661
Izod Impact Unnotched
63.0
J
Thermal Properties
Original Value
Comments
CTE, linear
10.5
µm/m-°C
@Temperature 20.0 - 100 °C
11.8
µm/m-°C
@Temperature 0.000 - 300 °C
12.5
µm/m-°C
@Temperature 0.000 - 500 °C
Processing Properties
Original Value
Comments
Processing Temperature
205
-
540
°C
Tempering Temperature
980
-
1025
°C
Hardening Temperature
Annealing Temperature
870
-
900
°C
Component Elements Properties
Original Value
Comments
Carbon, C
1.4 - 1.6 %
Chromium, Cr
11 - 13 %
Cobalt, Co
<= 1.0 %
Iron, Fe
80.8 - 86.9 %
As Balance
Manganese, Mn
<= 0.60 %
Molybdenum, Mo
0.70 - 1.2 %
Phosphorus, P
<= 0.030 %
Silicon, Si
<= 0.60 %
Sulfur, S
<= 0.030 %
Vanadium, V
<= 1.1 %
References
for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
AISI Type D2 Tool Steel, air quenched at 1010°C, tempered at 200°C
AISI Type D2 Tool Steel, air-quenched from 1010°C, tempered at 315°C
Bohler-Uddeholm AISI D2 Cold Work Tool Steel
AISI Type A2 Tool Steel
Crucible Steel AIRDI® 150 (AISI D2) Tool Steel
MSTD2C / 14253
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.