MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Zytel® HTN FR52G20NH BK337 Polyphthalamide (PPA)  (discontinued **)
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 20% Glass Fiber Reinforced

Material Notes: Zytel® HTNFR52G20NH BK337 is a 20% glass reinforced, flame retardant, lubricated high performance polyamide resin. It is also a PPA resin and it uses a non-halogenated flame retardant.

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.35 g/ccDAM; ISO 1183
Filler Content 20 %DAM
Linear Mold Shrinkage, Flow 0.0030 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.011 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 123 MPa
@Temperature 23.0 °C
50%RH; ISO 527
 135 MPa
@Temperature 23.0 °C
DAM; ISO 527
Elongation at Break 2.3 %
@Temperature 23.0 °C
50%RH; ISO 527
 2.4 %
@Temperature 23.0 °C
DAM; ISO 527
Tensile Modulus 8200 MPa
@Temperature 23.0 °C
DAM; ISO 527
 8600 MPa
@Temperature 23.0 °C
50%RH; ISO 527
Flexural Strength 180 MPa
@Temperature 23.0 °C
50%RH; ISO 178
 205 MPa
@Temperature 23.0 °C
DAM; ISO 178
Flexural Modulus 7300 MPa
@Temperature 23.0 °C
DAM; ISO 178
 8100 MPa
@Temperature 23.0 °C
50%RH; ISO 178
Charpy Impact Unnotched 30.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eU
 30.0 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 179/1eU
 30.0 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 179/1eU
 35.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 5.00 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 179/1eA
 5.00 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 179/1eA
 6.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 6.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 600 V
@Temperature 23.0 °C
DAM; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 21.0 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ISO 11359-1/-2
 25.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ISO 11359-1/-2
 27.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
 40.0 µm/m-°C
@Temperature 160 - 250 °C
DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 64.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
 68.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ISO 11359-1/-2
 100 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ISO 11359-1/-2
 130 µm/m-°C
@Temperature 160 - 250 °C
DAM; ISO 11359-1/-2
Melting Point 310 °C10°C/min, First Heat; DAM; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 276 °CDAM; ISO 75-1/-2
Flammability, UL94 V-0
@Thickness 3.00 mm
DAM; IEC 60695-11-10
 V-0
@Thickness 1.50 mm
DAM; IEC 60695-11-10
 V-0
@Thickness 0.750 mm
DAM; IEC 60695-11-10
 V-0
@Thickness 0.400 mm
DAM; IEC 60695-11-10
 V-0
@Thickness 0.400 mm
DAM; UL94
 V-0
@Thickness 1.50 mm
DAM; UL94
 V-0
@Thickness 3.00 mm
DAM; UL94
 V-0
@Thickness 0.750 mm
DAM; UL94
Oxygen Index 32 %DAM; ISO 4589-1/-2
Glow Wire Ignition Temperature 725 °C
@Thickness 0.400 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 0.400 mm
DAM; IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Melt Temperature 320 - 325 °CDAM
Mold Temperature 85.0 - 130 °CDAM
Drying Temperature 100 °CDAM
Dry Time 6.00 - 8.00 hourDAM
Moisture Content <= 0.10 %DAM
 
Descriptive Properties
AppearanceBlack ColorDAM
FillerGlass ReinforcedDAM
FormsPelletsDAM
GenericPolyphthalamide (PPA)DAM
Material StatusPreliminary DataDAM
Part Marking Code>PA6T/66-GF20FR<ISO 11469; DAM
 >PPA-GF20FR<SAE J1344; DAM
Polymer FamilyHigh performance polyamideDAM
Polymer TypePartially Aromatic PA, PPADAM
Processing MethodInjection MoldingDAM
Product CategoryFlame Retardant ResinsDAM
 Glass Reinforced ResinsDAM
Region Available - GlobalYesDAM
Resin IdentificationPA6T/66-GF20FRISO 1043; DAM

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Zytel® HTN 51G35NOX BK420 Polyphthalamide (PPA)
DuPont Mobility and Materials Zytel® HTN FR52G30NHF BK337 Polyphthalamide (PPA)
DuPont Mobility and Materials Zytel® HTN 52G45HSL NC010 Polyphthalamide (PPA)
DuPont Mobility and Materials Zytel® HTN 52G35HSL NC010 Polyphthalamide (PPA)
DuPont Mobility and Materials Zytel® HTN 92G45DH2 BK083 Polyphthalamide (PPA)

PZDSZ1446 / 140263

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.