MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont Teijin Films Melinex® ST504 Polyester Film, 500 Gauge
Categories: Polymer; Film; Thermoplastic; Polyester, TP; Polyester Film

Material Notes: Melinex® ST504 is a crystal clear, high gloss, heat stabilized polyester film. It can be overprinted with a wide range of solvent-based graphic inks and varnishes, silver conductive and dielectric inks. It is ideally suited for graphic and certain circuitry layers in membrane touch switches. Melinex® ST504 is pretreated on one side to promote adhesion.

Information provided by DuPont.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Thickness 5.00 mil
 
Mechanical PropertiesOriginal ValueComments
Flex Crack Resistance >= 20000Cycles; ASTM D2176
Coefficient of Friction, Static <= 0.60ASTM D1894
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+17 ohm-cmASTM D257
Surface Resistivity per Square 1.00e+13 ohmASTM D257
Dielectric Constant 2.9ASTM D150
Dielectric Strength 3000 V/milASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear 18.0 µm/m-°C
@Temperature 20.0 - 50.0 °C
Melting Point 493 °F
Shrinkage, MD 0.15 %
@Temperature 150 °C,
Time 1800 sec
Unrestrained
Shrinkage, TD 0.15 %
@Temperature 150 °C,
Time 1800 sec
Unrestrained
 
Optical PropertiesOriginal ValueComments
Haze 0.80 %ASTM D1003
Gloss 140 %60°; ASTM D1003
Transmission, Visible >= 85 %TLT; ASTM D1003
 
Descriptive Properties
Coefficient of Hygroscopic Expansion0.000006 IN/IN/% RH40% - 80% RH

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Teijin Films Melinex® ST329 Polyester Film, 1000 Gauge
DuPont Teijin Films Melinex® ST328 Polyester Film, 1400 Gauge
DuPont Teijin Films Melinex® S Polyester Film, 48 Gauge
DuPont Teijin Films Melinex® RFL1 Polyester Film, 600 Gauge
DuPont Teijin Films Melinex® HS2 Polyester Film

PDTZ9237 / 139565

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.