MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Meldin Supplier

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Vespel® SP-2515 Direct Formed (DF) Polyimide Parts
Categories: Polymer; Thermoplastic; Polyimide, Thermoplastic

Material Notes: Parts made from DuPont™ Vespel® SP-2515 offer a low coefficient of thermal expansion (CTE), excellent wear against both aluminum and steel alloys, and a low coefficient of friction in both dry and lubricated conditions. These properties make Vespel® SP-2515 parts ideal for applications such as seal rings, thrust washers, and bushings where high energy efficiency and dimensional stability, over a broad range of temperatures, are a requirement.

Information provided by DuPont. This product line has remained with DuPont after the DuPont-Dow merger.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.73 g/ccASTM D792
Water Absorption 0.30 %
@Time 86400 sec
ASTM D570
Deformation 0.090 %
@Time Error in fixSigDigits: @digits must be between 1 a sec,
Pressure 14.0 MPa
ASTM D621
 0.11 %
@Pressure 14.0 MPa,
Time 86400 sec
ASTM D621
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 25.0 MPa
@Temperature 260 °C
E-8 Specimen
 39.0 MPa
@Temperature 22.8 °C
ASTM D638
Elongation at Break 1.9 %
@Temperature 22.8 °C
ASTM D638
 2.1 %
@Temperature 260 °C
E-8 Specimen
Modulus of Elasticity 2.26 GPa
@Temperature 260 °C
E-8 Specimen
 6.34 GPa
@Temperature 22.8 °C
ASTM D638
Flexural Strength 38.0 MPa
@Temperature 260 °C
ASTM D790
 61.0 MPa
@Temperature 22.8 °C
ASTM D790
Flexural Modulus 3820 MPa
@Temperature 260 °C
ASTM D790
 5560 MPa
@Temperature 22.8 °C
ASTM D790
Compressive Strength 71.0 MPa
@Temperature 260 °C
ASTM D695
 105 MPa
@Temperature 22.8 °C
ASTM D695
Compressive Modulus 1840 MPa
@Temperature 260 °C
ASTM D695
 2080 MPa
@Temperature 22.8 °C
ASTM D695
Coefficient of Friction, Dynamic 0.21
@Pressure 1.30 MPa
0.88 PV, 0.7 m/s; Falex
 0.33
@Pressure 1.70 MPa
3.5 PV, 2 m/s; Falex
K (wear) Factor 74.0 x 10-10 in³-min/ft-lb-hr
@Pressure 1.29 MPa
25,000 psi-fpm PV; 0.7 m/s (134 fpm); Falex, Unlubicated
 282 x 10-10 in³-min/ft-lb-hr
@Pressure 1.72 MPa
100,000 psi-fpm PV; 2.0 m/s (400 fpm); Falex, Unlubicated
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.0 µm/m-°C
@Temperature 50.0 - 150 °C
Perpendicular; ASTM E831
 54.0 µm/m-°C
@Temperature 50.0 - 150 °C
Parallel; ASTM E831
Specific Heat Capacity 0.214 BTU/lb-°F
@Temperature 60.0 °C
ASTM E1269
Thermal Conductivity 2.04 W/m-K
@Temperature 100 °C
ASTM F433
 2.05 W/m-K
@Temperature 50.0 °C
ASTM F433

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Vespel® SP-1 ISO Polyimide
DuPont Mobility and Materials VESPEL TP-8054 Polyimide
DuPont Mobility and Materials VESPEL TP-8929 Polyimide
DuPont Mobility and Materials Vespel® CP-0644 Polyimide
DuPont Mobility and Materials Vespel® SP-221 DF Polyimide

PDTA7759m / 183713

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.