MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Coronze Copper, UNS C63800, H08 Temper sheet/strip
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent cold workability and hot formability.

Applications: springs, switch parts, contacts, relay springs, glass sealing and porcelain enameling.

Available as flat products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.28 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 100
Hardness, Rockwell 30T 83
Tensile Strength, Ultimate 900 MPaas rolled; strip
 490 MPa
@Treatment Temp. 700 °C
strip, annealed 1h
 520 MPa
@Treatment Temp. 600 °C
strip, annealed 1h
 560 MPa
@Treatment Temp. 500 °C
strip, annealed 1h
 605 MPa
@Treatment Temp. 400 °C
strip, annealed 1h
 905 MPa
@Treatment Temp. 300 °C
strip, annealed 1h
 930 MPa
@Treatment Temp. 200 °C
strip, annealed 1h
Tensile Strength, Yield 800 MPaas rolled; strip
 200 MPa
@Treatment Temp. 700 °C
strip, annealed 1h
 280 MPa
@Treatment Temp. 600 °C
strip, annealed 1h
 360 MPa
@Treatment Temp. 500 °C
strip, annealed 1h
 440 MPa
@Treatment Temp. 400 °C
strip, annealed 1h
 815 MPa
@Treatment Temp. 300 °C
strip, annealed 1h
 840 MPa
@Treatment Temp. 200 °C
strip, annealed 1h
 800 MPa
@Strain 0.2 %
Elongation at Break 3.0 %
 4.0 %as rolled; strip
 2.0 %
@Treatment Temp. 200 °C
strip, annealed 1h
 4.0 %
@Treatment Temp. 300 °C
strip, annealed 1h
 31 %
@Treatment Temp. 400 °C
strip, annealed 1h
 36 %
@Treatment Temp. 500 °C
strip, annealed 1h
 43 %
@Treatment Temp. 600 °C
strip, annealed 1h
 49 %
@Treatment Temp. 700 °C
strip, annealed 1h
Modulus of Elasticity 117 GPa
Poissons Ratio 0.312
Shear Modulus 45.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000174 ohm-cmAnnealed
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.1 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.375 J/g-°C
Thermal Conductivity 42.0 W/m-K
@Temperature 20.0 °C
Melting Point 1000 - 1030 °C
Solidus 1000 °C
Liquidus 1030 °C
Annealing Point 750 - 1100 °F
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 400 - 600 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 2.5 - 3.1 %
Cobalt, Co 0.25 - 0.55 %
Copper, Cu 95 %
Iron, Fe <= 0.10 %
Lead, Pb <= 0.050 %
Manganese, Mn <= 0.10 %
Nickel, Ni <= 0.10 %
Silicon, Si 1.5 - 2.1 %
Zinc, Zn <= 0.80 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
NAECO® ELKON® 2140C Copper Tungsten Nickel material
Beryllium Copper Nickel 72C Casting Alloy, Solution Treated and Aged
Coronze Copper, UNS C63800, H06 Temper sheet/strip
Overview of materials for Bronze
Copper, UNS C65400, H10 Temper strip

MC63800b8 / 11626

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.