MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Refractory Metals

(Viewing data as-entered. Click here to return)
Niobium, Nb (Columbium, Cb); Annealed Sample
Categories: Metal; Nonferrous Metal; Niobium Alloy; Refractory Metal; Pure Element

Material Notes: Annealed applies only to tensile and/or hardness values; other property values are typical of the element. The name niobium is used by chemists but the element is often called columbium by American metallurgists.

Fabrication: good formability, work hardens slowly, cannot be soldered. Joining requires adhesives, rivets, nuts and bolts, or capacitive discharge welding.

Applications: used in aerospace applications (i.e. rocket boosters), sodium vapor lamps, and superconductors.

Vendors: PLANSEE SE: Whether it's high temperatures, aggressive chemicals or extreme mechanical loading: PLANSEE supplies a suitable product solution in refractory metals or composite materials. As the world market leader in powder metallurgically produced high performance materials we combine outstanding materials knowledge with profound applications and technology know-how. Visit us at www.plansee.com.

Eagle Alloys Corporation is a leading supplier of quality metals and alloys. Our staff prides itself on working fast, efficiently and courteously to get you the information you need. Call (800) 237-9012 or visit www.EagleAlloys.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.60 g/cc
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 92.906381995
Atomic Number 41
Thermal Neutron Cross Section 1.1 barns/atom
X-ray Absorption Edge 0.65291 ÅK
 4.59111 ÅLI
 5.02472 ÅLII
 5.22596 ÅLIII
Electrode Potential -1.10 V
Electronegativity 1.6Pauling
Ionic Radius 0.690 ÅCrystal Ionic Radius for Valence +5
 0.740 ÅCrystal Ionic Radius for Valence +4
 1.00 ÅCrystal Ionic Radius for Valence +1
Electrochemical Equivalent 0.45 g/A/h
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 80
Tensile Strength 10.0 ksi
@Temperature 1090 °C
Recrystallized
Tensile Strength, Ultimate 300 MPa
Tensile Strength, Yield 207 MPa
Elongation at Break 30 %
Rupture Strength 5400 psi
@Temperature 1090 °C,
Time 36000 sec
Recrystallized
Modulus of Elasticity 103 GPa
Poissons Ratio 0.38
Shear Modulus 37.5 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000151 ohm-cm
Magnetic Susceptibility 0.00000228cgs/g
Critical Magnetic Field Strength, Oersted 2010 - 2110
Critical Superconducting Temperature 9.23 - 9.27 K
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 290 J/g
Heat of Vaporization 7704 J/g
CTE, linear 7.10 µm/m-°C
@Temperature 20.0 - 100 °C
 7.38 µm/m-°C
@Temperature 300 °C
 7.61 µm/m-°C
@Temperature 500 °C
 8.52 µm/m-°C
@Temperature 1000 °C
Specific Heat Capacity 0.272 J/g-°C
 0.3251 J/g-°CGas
Thermal Conductivity 52.3 W/m-K
@Temperature 20.0 °C
 54.4 W/m-K
@Temperature 100 °C
 56.5 W/m-K
@Temperature 200 °C
 58.6 W/m-K
@Temperature 300 °C
 60.7 W/m-K
@Temperature 400 °C
 63.2 W/m-K
@Temperature 500 °C
 65.3 W/m-K
@Temperature 600 °C
Melting Point 2468 °C
Boiling Point 4744 °C
Heat of Formation 0.000 kJ/molCrystal
 725.9 kJ/molGas
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.39
@Temperature 2000 °C
 0.78
@Temperature 1350 °C
 
Component Elements PropertiesOriginal ValueComments
Niobium, Nb (Columbium, Cb) 100 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Molybdenum, Mo, Annealed
Nickel, Ni
Aluminum, Al
Niobium, Nb (Columbium, Cb); Cold-Worked
Niobium, Nb (Columbium, Cb); Wrought

AMENb00 / 66

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.