MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

Nickel, Ni
Categories: Metal; Nonferrous Metal; Nickel Alloy; Pure Element

Material Notes: This entry is for pure Ni.

Nickel based alloys are the mainstay of many high performance markets in which corrosion resistance and/or heat resistance is required. Example applications include furnace components, chemical processing vessels, exchangers, and piping, high temperature aerospace components, nuclear reactors, extreme service pumps, turbines, pulp and paper production, and pollution control.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.88 g/cc0.321 lb/in³
 
Chemical PropertiesMetricEnglishComments
Atomic Mass 58.693458.69341995
Atomic Number 2828
Thermal Neutron Cross Section 4.8 barns/atom4.8 barns/atom
X-ray Absorption Edge 1.488 Å1.488 ÅK
 12.267 Å12.267 ÅLI
 14.135 Å14.135 ÅLII
 14.4476 Å14.4476 ÅLIII
Electrode Potential -0.250 V-0.250 V
Electronegativity 1.911.91Pauling
Ionic Radius 0.690 Å0.690 ÅCrystal Ionic Radius for Valence +2
Electrochemical Equivalent 1.0945 g/A/h1.0945 g/A/h
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 45.0 MPa6530 psiAnnealed
 317 MPa46000 psiTypical
Tensile Strength, Yield 59.0 MPa8560 psiTypical
Elongation at Break 30 %30 %Annealed
Modulus of Elasticity 207 GPa30000 ksi
Poissons Ratio 0.310.31
Shear Modulus 76.0 GPa11000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000640 ohm-cm0.00000640 ohm-cm
Magnetic Permeability 12401240mu(max) with B=1900G
Curie Temperature 358 °C676 °F
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 305.6 J/g131.5 BTU/lb
Heat of Vaporization 5862 J/g2522 BTU/lb
CTE, linear 13.1 µm/m-°C
@Temperature 20.0 °C
7.28 µin/in-°F
@Temperature 68.0 °F
Specific Heat Capacity 0.460 J/g-°C0.110 BTU/lb-°F
Thermal Conductivity 60.7 W/m-K421 BTU-in/hr-ft²-°F
Melting Point 1455 °C2651 °F
Boiling Point 2913 °C5275 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1)  0.080
@Temperature 200 - 400 °C
0.080
@Temperature 392 - 752 °F
polished total spectrum
 0.19
@Temperature 1000 °C
0.19
@Temperature 1830 °F
unoxidized
Reflection Coefficient, Visible (0-1) 0.4130.413300 nm spectral
 
Component Elements PropertiesMetricEnglishComments
Nickel, Ni 100 %100 %
 
Descriptive Properties
CAS Number7440-02-0

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum, Al
Iron, Fe
Gold, Au
Titanium, Ti
Copper, Cu; Annealed

AMENi00 / 71

Metalmen Sales
metalmen Is Your Direct to US Manufacturing Source for High Purity Metals

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.