MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
High-leaded brass, UNS C34200, OSO35 Temper flat products
Categories: Metal; Nonferrous Metal; Copper Alloy; Brass

Material Notes: Fair to excellent corrosion resistance. Combines excellent machinability with moderate cold workability.

Applications: gears, wheels, nuts, plates for clocks, keys, bearing cages, engraver's plates.

Test specimen: flat product - 1mm thickness.

Key Words: CZ119, ISO CuZn35Pb2, CEN CW601N, free-cutting brass
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.50 g/cc
Grain Size 7.0 µm
@Treatment Temp. 300 °C
thick strip cold rolled
 13 µm
@Treatment Temp. 400 °C
thick strip cold rolled
 25 µm
@Treatment Temp. 500 °C
thick strip cold rolled
 53 µm
@Treatment Temp. 600 °C
thick strip cold rolled
 100 µm
@Treatment Temp. 700 °C
thick strip cold rolled
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell F 68
Hardness, Rockwell 30T 32
Tensile Strength, Ultimate 340 MPa
 290 MPa
@Treatment Temp. 700 °C
thick strip cold rolled
 325 MPa
@Treatment Temp. 600 °C
thick strip cold rolled
 360 MPa
@Treatment Temp. 500 °C
thick strip cold rolled
 395 MPa
@Treatment Temp. 400 °C
thick strip cold rolled
 570 MPa
@Treatment Temp. 300 °C
thick strip cold rolled
 600 MPa
@Treatment Temp. 200 °C
thick strip cold rolled
Tensile Strength, Yield 115 MPa
@Strain 0.5 %
Elongation at Break 52 %In 50 mm
 6.0 %
@Treatment Temp. 200 °C
thick strip cold rolled
 13 %
@Treatment Temp. 300 °C
thick strip cold rolled
 41 %
@Treatment Temp. 400 °C
thick strip cold rolled
 51 %
@Treatment Temp. 500 °C
thick strip cold rolled
 55 %
@Treatment Temp. 600 °C
thick strip cold rolled
 57 %
@Treatment Temp. 700 °C
thick strip cold rolled
Modulus of Elasticity 105 GPa
Poissons Ratio 0.346
Machinability 90 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 39.0 GPa
Shear Strength 235 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000660 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 20.3 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.380 J/g-°C
Thermal Conductivity 115 W/m-K
@Temperature 20.0 °C
Melting Point 885 - 910 °C
Solidus 885 °C
Liquidus 910 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 425 - 600 °C
Hot-Working Temperature 785 - 815 °C
Recrystallization Temperature 320 °C
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 62.5 - 66.5 %
Iron, Fe <= 0.10 %
Lead, Pb 1.5 - 2.5 %
Other, total <= 0.50 %
Zinc, Zn 33.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
High-leaded brass, UNS C34200, OSO15 Temper flat products
High-leaded brass, UNS C34200, OSO25 Temper flat products
Phosphor bronze 10% Sn, UNS C52400, H01 Temper wire
Phosphor bronze 10% Sn, UNS C52400, OSO35 Temper flat products
Phosphor bronze 8% Sn, UNS C52100

MC34200b4 / 11203

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.