Physical Properties | Metric | English | Comments |
---|
Density | 7.90 g/cc | 0.285 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Vickers | 160 @Thickness 4.00 mm | 160 @Thickness 0.157 in |
| 180 @Thickness 1.00 mm | 180 @Thickness 0.0394 in |
Tensile Strength, Ultimate | 58.0 MPa @Temperature 1000 °C | 8410 psi @Temperature 1830 °F |
| 95.0 MPa @Temperature 900 °C | 13800 psi @Temperature 1650 °F |
| 170 MPa @Temperature 800 °C | 24700 psi @Temperature 1470 °F |
| 650 MPa @Thickness 4.00 mm | 94300 psi @Thickness 0.157 in |
| 675 MPa @Thickness 1.00 mm | 97900 psi @Thickness 0.0394 in |
Tensile Strength, Yield | 300 MPa @Strain 0.2 %, Thickness 4.00 mm | 43500 psi @Strain 0.2 %, Thickness 0.157 in |
| 340 MPa @Strain 0.2 %, Thickness 1.00 mm | 49300 psi @Strain 0.2 %, Thickness 0.0394 in |
Elongation at Break | 30 % @Thickness 4.00 mm | 30 % @Thickness 0.157 in |
| 35 % @Thickness 1.00 mm | 35 % @Thickness 0.0394 in |
Creep Strength | 4.00 MPa @Temperature 1000 °C, Time 3.60e+6 sec | 580 psi @Temperature 1830 °F, Time 1000 hour |
| 20.0 MPa @Temperature 800 °C, Time 3.60e+6 sec | 2900 psi @Temperature 1470 °F, Time 1000 hour |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000104 ohm-cm | 0.000104 ohm-cm |
| 0.000107 ohm-cm @Temperature 100 °C | 0.000107 ohm-cm @Temperature 212 °F |
| 0.000110 ohm-cm @Temperature 200 °C | 0.000110 ohm-cm @Temperature 392 °F |
| 0.000114 ohm-cm @Temperature 300 °C | 0.000114 ohm-cm @Temperature 572 °F |
| 0.000116 ohm-cm @Temperature 400 °C | 0.000116 ohm-cm @Temperature 752 °F |
| 0.000119 ohm-cm @Temperature 500 °C | 0.000119 ohm-cm @Temperature 932 °F |
| 0.000121 ohm-cm @Temperature 600 °C | 0.000121 ohm-cm @Temperature 1110 °F |
| 0.000123 ohm-cm @Temperature 700 °C | 0.000123 ohm-cm @Temperature 1290 °F |
| 0.000125 ohm-cm @Temperature 800 °C | 0.000125 ohm-cm @Temperature 1470 °F |
| 0.000126 ohm-cm @Temperature 900 °C | 0.000126 ohm-cm @Temperature 1650 °F |
| 0.000128 ohm-cm @Temperature 1000 °C | 0.000128 ohm-cm @Temperature 1830 °F |
| 0.000129 ohm-cm @Temperature 1100 °C | 0.000129 ohm-cm @Temperature 2010 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 16.0 µm/m-°C @Temperature 20.0 - 250 °C | 8.89 µin/in-°F @Temperature 68.0 - 482 °F |
| 17.0 µm/m-°C @Temperature 20.0 - 500 °C | 9.44 µin/in-°F @Temperature 68.0 - 932 °F |
| 18.0 µm/m-°C @Temperature 20.0 - 750 °C | 10.0 µin/in-°F @Temperature 68.0 - 1380 °F |
| 19.0 µm/m-°C @Temperature 20.0 - 1000 °C | 10.6 µin/in-°F @Temperature 68.0 - 1830 °F |
Specific Heat Capacity | 0.500 J/g-°C @Temperature 20.0 °C | 0.120 BTU/lb-°F @Temperature 68.0 °F |
| 0.500 J/g-°C @Temperature 100 °C | 0.120 BTU/lb-°F @Temperature 212 °F |
| 0.500 J/g-°C @Temperature 200 °C | 0.120 BTU/lb-°F @Temperature 392 °F |
| 0.510 J/g-°C @Temperature 300 °C | 0.122 BTU/lb-°F @Temperature 572 °F |
| 0.540 J/g-°C @Temperature 400 °C | 0.129 BTU/lb-°F @Temperature 752 °F |
| 0.570 J/g-°C @Temperature 500 °C | 0.136 BTU/lb-°F @Temperature 932 °F |
| 0.600 J/g-°C @Temperature 600 °C | 0.143 BTU/lb-°F @Temperature 1110 °F |
| 0.620 J/g-°C @Temperature 700 °C | 0.148 BTU/lb-°F @Temperature 1290 °F |
| 0.640 J/g-°C @Temperature 800 °C | 0.153 BTU/lb-°F @Temperature 1470 °F |
| 0.670 J/g-°C @Temperature 900 °C | 0.160 BTU/lb-°F @Temperature 1650 °F |
| 0.700 J/g-°C @Temperature 1000 °C | 0.167 BTU/lb-°F @Temperature 1830 °F |
| 0.730 J/g-°C @Temperature 1100 °C | 0.174 BTU/lb-°F @Temperature 2010 °F |
Thermal Conductivity | 13.0 W/m-K @Temperature 20.0 °C | 90.2 BTU-in/hr-ft²-°F @Temperature 68.0 °F |
| 14.0 W/m-K @Temperature 100 °C | 97.2 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 15.0 W/m-K @Temperature 200 °C | 104 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 16.0 W/m-K @Temperature 300 °C | 111 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 18.0 W/m-K @Temperature 400 °C | 125 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 19.0 W/m-K @Temperature 500 °C | 132 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 21.0 W/m-K @Temperature 600 °C | 146 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 22.0 W/m-K @Temperature 700 °C | 153 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 24.0 W/m-K @Temperature 800 °C | 167 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 25.0 W/m-K @Temperature 900 °C | 174 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 26.0 W/m-K @Temperature 1000 °C | 180 BTU-in/hr-ft²-°F @Temperature 1830 °F |
| 28.0 W/m-K @Temperature 1100 °C | 194 BTU-in/hr-ft²-°F @Temperature 2010 °F |
Melting Point | 1390 °C | 2530 °F |
Maximum Service Temperature, Air | 1100 °C | 2010 °F |
|
Optical Properties | Metric | English | Comments |
---|
Emissivity (0-1) | 0.88 | 0.88 |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | <= 0.10 % | <= 0.10 % |
Chromium, Cr | 18 - 21 % | 18 - 21 % |
Iron, Fe | >= 38.4 % | >= 38.4 % |
Manganese, Mn | <= 1.0 % | <= 1.0 % |
Nickel, Ni | 34 - 37 % | 34 - 37 % |
Silicon, Si | 1.6 - 2.5 % | 1.6 - 2.5 % |