MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Sipchem PBT-R1-E0-020
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Unreinforced, Molded

Material Notes: Product description: Sipchem PBT-R1-E0-020 is a Polybutylene Terephthalate resin, manufactured by Sipchem Chemical Company in The Kingdom of Saudi Arabia using an Inventa-Fischer Technology. PBT-R1-E0-020 is a medium viscosity neat PBT resin

Applications: Compounding

Information provided by Sahara International Petrochemical Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.31 g/cc0.0473 lb/in³ASTM D1505
Viscosity Number 110 cm³/g1.1 dl/gIntrinsic; ASTM D2857
Melt Flow 20 g/10 min
@Load 2.16 kg,
Temperature 250 °C
20 g/10 min
@Load 4.76 lb,
Temperature 482 °F
ASTM D1238
 
Chemical PropertiesMetricEnglishComments
Carboxyl End Groups <= 30 meq/kg<= 30 meq/kgISO 2114
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 57.9 MPa8400 psiASTM D638
Elongation at Yield 3.6 %3.6 %ASTM D638
Flexural Strength 81.8 MPa11900 psiASTM D790
Flexural Modulus 2.18 GPa316 ksiASTM D790
Flexural Strain at Yield 8.4 %8.4 %at Flexural Strength; ASTM D790
Izod Impact, Notched 0.271 J/cm0.508 ft-lb/inASTM D256
Izod Impact, Unnotched NBNBASTM D256
 
Thermal PropertiesMetricEnglishComments
Melting Point 223 °C433 °FASTM D3418
Deflection Temperature at 1.8 MPa (264 psi) 50.5 °C123 °FASTM D648
Vicat Softening Point 173.4 °C344.1 °FASTM D1525
Flammability, UL94 HBHBIEC 60695
 
Descriptive Properties
Color<3(b*), ASTM D6290

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSIPCH027 / 285340

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.