MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Teknor Apex Sarlink® TPV X4750B42 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 4700 Series are a very high flow injection molded engineering grades with excellent UV resistance, elasticity, and surface aesthetics designed for demanding automotive applications including window encapsulation and exterior parts. This product is a black, medium hardness, low density thermoplastic vulcanizate suited for injection molding applications that require superior flow properties.

Availability: Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Good Processability; High Flow; High Heat Resistance; Low Compression Set; Low Density; Low Specific Gravity; Medium Hardness; Resilient; UV Resistant

Uses: Automotive Applications; Automotive Exterior Parts; Automotive Window Encapsulation; Rubber Replacement

RoHS Compliance: RoHS Compliant

Automotive Specifications: CHRYSLER MS-AR-100 AMV Color: Natural; GM GMP.E/P.078 Color: Natural; GM GMW15812P-TPV (EPDM=PP) Type 4M Color: Natural; GM Sarlink Color

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.910 g/ccISO 1183
Viscosity 220 cP
@Shear Rate 206 1/s,
Temperature 200 °C
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 50
@Time 5.00 sec
Extruded; ISO 868
 53
@Time 5.00 sec
Injection Molded; ISO 868
Tensile Strength at Break 566 psiFlow; ISO 37
 609 psiAcross Flow; ISO 37
 542 psi
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
Across Flow, Change in Air at 168 hr; ISO 188
 731 psi
@Treatment Temp. 150 °C,
Time 605000 sec
Across Flow, Change in Air at 168 hr; ISO 188
Tensile Stress at Strain 218 psi
@Strain 100 %
Across Flow; ISO 37
 319 psi
@Strain 100 %
Flow; ISO 37
 203 psi
@Strain 100 %,
Treatment Temp. 150 °C
Across Flow, Change in Air at 168 hr; ISO 188
 216 psi
@Strain 100 %,
Treatment Temp. 135 °C
Across Flow, Change in Air at 1000 hr; ISO 188
Elongation at Break 320 %Flow; ISO 37
 440 %Across Flow; ISO 37
 383 %
@Treatment Temp. 150 °C,
Time 605000 sec
Across Flow, Change in Air at 168 hr; ISO 188
 436 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
Across Flow, Change in Air at 168 hr; ISO 188
Tear Strength 91.0 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set 15 %
@Temperature 22.8 °C,
Time 79200 sec
ISO 815
 26 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 40 %
@Temperature 125 °C,
Time 252000 sec
ISO 815
 
Processing PropertiesOriginal ValueComments
Processing Temperature 360 - 430 °FInjection, Melt
Rear Barrel Temperature 350 - 420 °FInjection
Middle Barrel Temperature 350 - 420 °FInjection
Front Barrel Temperature 350 - 420 °FInjection
Nozzle Temperature 370 - 430 °FInjection
Mold Temperature 50.0 - 150 °FInjection
Drying Temperature 180 °F
Dry Time 3.00 hour
Back Pressure 10.0 - 150 psiInjection
Screw Speed 100 - 200 rpmInjection
 
Descriptive Properties
AppearanceBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Teknor Apex Sarlink® TPV 5790B Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV X5735B Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 5765B Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 5755B Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 4785B40 Thermoplastic Vulcanizate

PTEKNQ1205 / 237696

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.