MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Daikin DAI-EL® G-9074 Fluoroelastomer Terpolymer, 71% Fluorine Content
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: DAI-EL® G-9074 is a medium viscosity, peroxide curable terpolymer designed especially for injection molding. It provides excellent mold flow and easy removal of molded parts. Properly compounded and cured, DAI-EL G-9074 has excellent compression set and chemical and steam resistance.

Typical Applications: O-Rings and seals

Rheological Properties MDR 2000:
Temperature: 177°C
Frequency: 100 cpm
Strain: 0.5°
Test time: 6 min

Rheological Properties ODR:
Temperature: 177°C
Frequency: 100 cpm
Strain: 3 °
Test time: 12 min

Information provided by Daikin.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.83 g/cc1.83 g/cc
Mooney Viscosity 42
@Temperature 121 °C
42
@Temperature 250 °F
ML 1+10
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6666
Tensile Strength at Break 18.5 MPa2680 psi
Elongation at Break 262 %262 %
100% Modulus 3.60 MPa
@Strain 100 %
522 psi
@Strain 100 %
Compression Set 10.8 %
@Temperature 200 °C,
Time 252000 sec
10.8 %
@Temperature 392 °F,
Time 70.0 hour
P24 O-ring; ASTM D395 Method B
 
Thermal PropertiesMetricEnglishComments
Minimum Service Temperature, Air -8.00 °C17.6 °FLow Temperature Retraction, TR10
 
Processing PropertiesMetricEnglishComments
Cure Time 0.700 min0.0117 hourts2, scorch time, MDR 2000
 0.930 min0.0155 hourt'50, time to 50% cure, MDR 2000
 1.33 min0.0222 hourts2, scorch time, ODR
 1.37 min0.0228 hourt'90, time to 90% cure, MDR 2000
 2.50 min0.0417 hourt'50, time to 50% cure, ODR
 3.32 min0.0553 hourt'90, time to 90% cure, ODR
 10.0 min
@Temperature 177 °C
0.167 hour
@Temperature 351 °F
Press Cure
 0.000 - 240 min
@Temperature 200 °C
0.000 - 4.00 hour
@Temperature 392 °F
Post cure
 
Component Elements PropertiesMetricEnglishComments
Fluorine, F 71 %71 %
 
Descriptive Properties
ColorWhite to cream
MH123.8 dNmmaximum torque, ODR
 23.2 dNmmaximum torque, MDR 2000
ML0.7 dNmminimum torque, MDR 2000
 7.7 dNmminimum torque, ODR
Test Formula1.5 phrPeroxide
 100 phrDAI-EL® G-9074
 20 phrMT Carbon Black (N-990)
 3 phrTAIC 70%

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AGC Lumiflon LF-600X Solvent Soluble Fluoropolymer

PDAIJ9862 / 209933

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.