MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Carpenter Gall-Tough PLUS™ Stainless, Annealed at 1066°C
Categories: Metal; Ferrous Metal; Stainless Steel

Material Notes: Data provided by Carpenter Technology Corporation.

6.4 mm diameter tensile specimens from center of 25.4 mm diameter bar annealed 1066°C 1 hour, water quenched, and ground.

Threshold Galling Stress 48 MPa. The avg. total volume loss on the wear test is 10.6 mm³ at 100 rpm.

Gall-Tough PLUS™ stainless is a high silicon, high manganese, nitrogen strengthened, austenitic stainless alloy which exhibits superior self-mated galling resistance and metal-to-metal wear resistance. The alloy possesses higher strength than Type 316. It also exhibits chloride corrosion resistance equal to or better then Type 316, along with equivalent high temperature oxidation resistance.

Gall-Tough PLUS™ is a trademark of Carpenter Technology Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.60 g/cc0.275 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 90 - 9590 - 95Typical
Tensile Strength, Ultimate 783 MPa114000 psi
 160 MPa
@Temperature 871 °C
23200 psi
@Temperature 1600 °F
 492 MPa
@Temperature 649 °C
71400 psi
@Temperature 1200 °F
 603 MPa
@Temperature 427 °C
87500 psi
@Temperature 801 °F
 638 MPa
@Temperature 204 °C
92500 psi
@Temperature 399 °F
Tensile Strength, Yield 423 MPa
@Strain 0.2 %
61400 psi
@Strain 0.2 %
 146 MPa
@Strain 0.2 %,
Temperature 871 °C
21200 psi
@Strain 0.2 %,
Temperature 1600 °F
 201 MPa
@Strain 0.2 %,
Temperature 649 °C
29200 psi
@Strain 0.2 %,
Temperature 1200 °F
 208 MPa
@Strain 0.2 %,
Temperature 427 °C
30200 psi
@Strain 0.2 %,
Temperature 801 °F
 222 MPa
@Strain 0.2 %,
Temperature 204 °C
32200 psi
@Strain 0.2 %,
Temperature 399 °F
Elongation at Break 59 %59 %in 4D
 48 %
@Temperature 649 °C
48 %
@Temperature 1200 °F
in 4D
 58 %
@Temperature 427 °C
58 %
@Temperature 801 °F
in 4D
 63 %
@Temperature 204 °C
63 %
@Temperature 399 °F
in 4D
 124 %
@Temperature 871 °C
124 %
@Temperature 1600 °F
in 4D
Reduction of Area 72 %72 %
 60 %
@Temperature 649 °C
60 %
@Temperature 1200 °F
 70 %
@Temperature 427 °C
70 %
@Temperature 801 °F
 73 %
@Temperature 204 °C
73 %
@Temperature 399 °F
 93 %
@Temperature 871 °C
93 %
@Temperature 1600 °F
Modulus of Elasticity 184.9 GPa26820 ksi
Fatigue Strength 293 MPa
@# of Cycles 1.00e+7
42500 psi
@# of Cycles 1.00e+7
rotating beam
Charpy Impact 404 J298 ft-lbTypical V-Notch
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000947 ohm-cm0.0000947 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  14.19 µm/m-°C
@Temperature 25.0 - 50.0 °C
7.883 µin/in-°F
@Temperature 77.0 - 122 °F
 17.1 µm/m-°C
@Temperature 25.0 - 250 °C
9.48 µin/in-°F
@Temperature 77.0 - 482 °F
 18.07 µm/m-°C
@Temperature 25.0 - 500 °C
10.04 µin/in-°F
@Temperature 77.0 - 932 °F
Specific Heat Capacity 0.5055 J/g-°C
@Temperature 50.0 - 100 °C
0.1208 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity 12.0 W/m-K83.3 BTU-in/hr-ft²-°F
 14.79 W/m-K
@Temperature 200 °C
102.6 BTU-in/hr-ft²-°F
@Temperature 392 °F
 18.9 W/m-K
@Temperature 400 °C
131 BTU-in/hr-ft²-°F
@Temperature 752 °F
 20.34 W/m-K
@Temperature 500 °C
141.2 BTU-in/hr-ft²-°F
@Temperature 932 °F
Maximum Service Temperature, Air 982 °C1800 °FScaling Temperature for Continuous Service
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.15 %<= 0.15 %
Chromium, Cr 16.5 - 21 %16.5 - 21 %
Iron, Fe 62 %62 %as remainder
Manganese, Mn 4.0 - 8.0 %4.0 - 8.0 %
Molybdenum, Mo 0.50 - 2.5 %0.50 - 2.5 %
Nickel, Ni 6.0 - 10 %6.0 - 10 %
Nitrogen, N 0.050 - 0.35 %0.050 - 0.35 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si 2.5 - 4.5 %2.5 - 4.5 %
Sulfur, S <= 0.040 %<= 0.040 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type S21800 Stainless Steel
Crucible Steel 303 SE Chromium-Nickel Steel
Crucible Steel 303 Plus Chromium-Nickel Steel
Titanium Ti-6Al-2Sn-4Zr-2Mo-0.1Si; Duplex Annealed
Alcoa Deltalloy® 4032-T86 Aluminum

NCAR1C / 15598

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.