MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Polyphthalamide (PPA), Mineral Filled
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), Mineral Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyphthalamide, Mineral Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.28 - 1.80 g/ccAverage value: 1.51 g/cc Grade Count:17
Water Absorption 0.100 - 0.200 %Average value: 0.134 % Grade Count:7
Moisture Absorption at Equilibrium 0.160 - 1.40 %Average value: 0.424 % Grade Count:5
Linear Mold Shrinkage 0.00300 - 0.0150 cm/cmAverage value: 0.00848 cm/cm Grade Count:12
Linear Mold Shrinkage, Transverse 0.00450 - 0.0110 cm/cmAverage value: 0.00853 cm/cm Grade Count:9
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 125 - 126Average value: 125 Grade Count:6
Tensile Strength, Ultimate 70.0 - 130 MPaAverage value: 100 MPa Grade Count:12
 24.1 - 115 MPa
@Temperature 60.0 - 175 °C
Average value: 63.2 MPa Grade Count:2
Tensile Strength, Yield 71.0 - 174 MPaAverage value: 111 MPa Grade Count:5
 20.0 - 97.0 MPa
@Temperature 100 - 175 °C
Average value: 46.2 MPa Grade Count:2
Elongation at Break 1.20 - 4.00 %Average value: 1.78 % Grade Count:15
 1.70 - 15.0 %
@Temperature 60.0 - 175 °C
Average value: 6.52 % Grade Count:4
Elongation at Yield 1.80 - 2.50 %Average value: 2.15 % Grade Count:4
Modulus of Elasticity 4.40 - 11.6 GPaAverage value: 8.40 GPa Grade Count:15
 0.600 - 8.70 GPa
@Temperature 60.0 - 175 °C
Average value: 3.81 GPa Grade Count:4
Flexural Yield Strength 110 - 263 MPaAverage value: 177 MPa Grade Count:15
 15.0 - 155 MPa
@Temperature 100 - 175 °C
Average value: 59.6 MPa Grade Count:3
Flexural Modulus 3.51 - 10.8 GPaAverage value: 6.89 GPa Grade Count:15
 0.600 - 6.80 GPa
@Temperature 100 - 175 °C
Average value: 2.69 GPa Grade Count:3
Compressive Yield Strength 152 - 185 MPaAverage value: 166 MPa Grade Count:3
Poissons Ratio 0.290 - 0.380Average value: 0.318 Grade Count:5
Shear Modulus 2.20 - 4.20 GPaAverage value: 3.23 GPa Grade Count:5
Shear Strength 69.0 - 96.0 MPaAverage value: 85.7 MPa Grade Count:8
Izod Impact, Notched 0.310 - 5.30 J/cmAverage value: 0.826 J/cm Grade Count:12
Izod Impact, Unnotched 3.47 - 7.47 J/cmAverage value: 5.92 J/cm Grade Count:5
Izod Impact, Notched (ISO) 2.90 - 95.0 kJ/m²Average value: 19.6 kJ/m² Grade Count:6
 4.00 - 4.00 kJ/m²
@Temperature -30.0 - -30.0 °C
Average value: 4.00 kJ/m² Grade Count:1
Izod Impact, Unnotched (ISO) 31.0 kJ/m² - NBAverage value: 42.0 kJ/m² Grade Count:3
 23.0 - 23.0 kJ/m²
@Temperature -5.00 - -5.00 °C
Average value: 23.0 kJ/m² Grade Count:1
Charpy Impact Unnotched 1.00 - 10.5 J/cm²Average value: 4.38 J/cm² Grade Count:6
 8.00 - 8.00 J/cm²
@Temperature -40.0 - -40.0 °C
Average value: 8.00 J/cm² Grade Count:1
Charpy Impact, Notched 0.200 - 0.800 J/cm²Average value: 0.400 J/cm² Grade Count:6
 0.500 - 0.500 J/cm²
@Temperature -40.0 - -40.0 °C
Average value: 0.500 J/cm² Grade Count:1
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+15 - 1.00e+16 ohm-cmAverage value: 6.14e+15 ohm-cm Grade Count:6
Dielectric Constant 3.90 - 4.70Average value: 4.22 Grade Count:6
Dissipation Factor 0.00500 - 0.0220Average value: 0.0123 Grade Count:6
Arc Resistance 120 - 125 secAverage value: 124 sec Grade Count:4
Comparative Tracking Index 550 VAverage value: 550 V Grade Count:7
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.0 - 41.0 µm/m-°CAverage value: 31.8 µm/m-°C Grade Count:4
 17.0 - 95.0 µm/m-°C
@Temperature 50.0 - 250 °C
Average value: 47.2 µm/m-°C Grade Count:5
CTE, linear, Transverse to Flow 40.0 - 80.0 µm/m-°CAverage value: 53.8 µm/m-°C Grade Count:4
 63.0 - 150 µm/m-°C
@Temperature 50.0 - 250 °C
Average value: 109 µm/m-°C Grade Count:4
Melting Point 265 - 324 °CAverage value: 308 °C Grade Count:10
Maximum Service Temperature, Air 130 - 150 °CAverage value: 140 °C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 158 - 306 °CAverage value: 265 °C Grade Count:9
Deflection Temperature at 1.8 MPa (264 psi) 80.0 - 279 °CAverage value: 184 °C Grade Count:12
Flammability, UL94 HBGrade Count:8
 
Processing PropertiesOriginal ValueComments
Melt Temperature 300 - 343 °CAverage value: 323 °C Grade Count:11
Mold Temperature 66.0 - 180 °CAverage value: 131 °C Grade Count:11
Drying Temperature 80.0 - 130 °CAverage value: 111 °C Grade Count:10
Moisture Content 0.0300 - 0.200 %Average value: 0.0693 % Grade Count:7
Dew Point -31.7 °CAverage value: -31.7 °C Grade Count:3
Injection Pressure 68.9 - 124 MPaAverage value: 96.5 MPa Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polyphthalamide (PPA), 30% Glass Fiber Reinforced
Overview of materials for Polyphthalamide (PPA)
Overview of materials for Polyphthalamide (PPA), 50% Glass Fiber Reinforced
Overview of materials for Polyphthalamide (PPA), Glass/PTFE
Overview of materials for Polyphthalamide (PPA), 40% Glass Fiber Reinforced

O4630 / 78368

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.