MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polyphthalamide (PPA), 50% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 50% Glass Fiber Reinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyphthalamide, 50% Glass Fiber Reinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.45 - 1.99 g/cc0.0524 - 0.0719 lb/in³Average value: 1.63 g/cc Grade Count:93
 1.10 - 1.10 g/cc
@Temperature 325 - 325 °C
0.0397 - 0.0397 lb/in³
@Temperature 617 - 617 °F
Average value: 1.10 g/cc Grade Count:1
Filler Content 45.0 - 50.0 %45.0 - 50.0 %Average value: 48.8 % Grade Count:28
Water Absorption 0.0200 - 4.00 %0.0200 - 4.00 %Average value: 0.360 % Grade Count:21
Moisture Absorption at Equilibrium 0.200 - 2.00 %0.200 - 2.00 %Average value: 1.28 % Grade Count:28
 0.850 - 0.950 %
@Temperature 70.0 - 70.0 °C
0.850 - 0.950 %
@Temperature 158 - 158 °F
Average value: 0.900 % Grade Count:8
Water Absorption at Saturation 2.50 - 4.30 %2.50 - 4.30 %Average value: 3.38 % Grade Count:10
Linear Mold Shrinkage 0.000100 - 0.00600 cm/cm0.000100 - 0.00600 in/inAverage value: 0.00229 cm/cm Grade Count:68
Linear Mold Shrinkage, Transverse 0.00100 - 0.0100 cm/cm0.00100 - 0.0100 in/inAverage value: 0.00591 cm/cm Grade Count:56
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 124 - 126124 - 126Average value: 125 Grade Count:9
Ball Indentation Hardness 340 - 360 MPa49300 - 52200 psiAverage value: 353 MPa Grade Count:3
Tensile Strength, Ultimate 70.0 - 295 MPa10200 - 42800 psiAverage value: 235 MPa Grade Count:87
 42.0 - 340 MPa
@Temperature -40.0 - 250 °C
6090 - 49300 psi
@Temperature -40.0 - 482 °F
Average value: 153 MPa Grade Count:15
Tensile Strength, Yield 24.8 - 260 MPa3600 - 37700 psiAverage value: 211 MPa Grade Count:7
Elongation at Break 0.600 - 3.20 %0.600 - 3.20 %Average value: 2.17 % Grade Count:92
 1.60 - 10.0 %
@Temperature -40.0 - 200 °C
1.60 - 10.0 %
@Temperature -40.0 - 392 °F
Average value: 3.84 % Grade Count:11
Modulus of Elasticity 10.3 - 22.1 GPa1490 - 3200 ksiAverage value: 17.4 GPa Grade Count:87
 1.10 - 19.0 GPa
@Temperature -40.0 - 200 °C
160 - 2760 ksi
@Temperature -40.0 - 392 °F
Average value: 12.2 GPa Grade Count:15
Flexural Yield Strength 177 - 440 MPa25700 - 63800 psiAverage value: 350 MPa Grade Count:62
 94.5 - 267 MPa
@Temperature 100 - 175 °C
13700 - 38700 psi
@Temperature 212 - 347 °F
Average value: 158 MPa Grade Count:1
Flexural Modulus 10.4 - 21.0 GPa1510 - 3040 ksiAverage value: 16.2 GPa Grade Count:68
 4.70 - 16.7 GPa
@Temperature 100 - 200 °C
682 - 2420 ksi
@Temperature 212 - 392 °F
Average value: 8.80 GPa Grade Count:5
Flexural Strain at Break 2.30 - 3.00 %2.30 - 3.00 %Average value: 2.57 % Grade Count:6
Compressive Yield Strength 168 - 314 MPa24400 - 45500 psiAverage value: 212 MPa Grade Count:4
Poissons Ratio 0.330 - 0.4100.330 - 0.410Average value: 0.351 Grade Count:10
Fatigue Strength  100 - 100 MPa
@# of Cycles 1580 - 1580
14500 - 14500 psi
@# of Cycles 1580 - 1580
Average value: 100 MPa Grade Count:1
 100 - 100 MPa
@Temperature 140 - 140 °C
14500 - 14500 psi
@Temperature 284 - 284 °F
Average value: 100 MPa Grade Count:1
Shear Modulus 0.350 - 4.00 GPa
@Temperature 0.000 - 350 °C
50.8 - 580 ksi
@Temperature 32.0 - 662 °F
Average value: 1.75 GPa Grade Count:3
Shear Strength 89.6 - 108 MPa13000 - 15700 psiAverage value: 99.2 MPa Grade Count:4
Izod Impact, Notched 0.590 - 4.97 J/cm1.11 - 9.30 ft-lb/inAverage value: 1.36 J/cm Grade Count:25
Izod Impact, Unnotched 3.86 - 13.0 J/cm7.23 - 24.4 ft-lb/inAverage value: 8.84 J/cm Grade Count:13
Izod Impact, Notched (ISO) 7.80 - 17.0 kJ/m²3.71 - 8.09 ft-lb/in²Average value: 11.9 kJ/m² Grade Count:24
 11.0 - 13.5 kJ/m²
@Temperature -40.0 - -20.0 °C
5.23 - 6.42 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 12.1 kJ/m² Grade Count:7
Izod Impact, Unnotched (ISO) 42.0 - 87.0 kJ/m²20.0 - 41.4 ft-lb/in²Average value: 61.1 kJ/m² Grade Count:10
 50.0 - 69.0 kJ/m²
@Temperature -30.0 - -30.0 °C
23.8 - 32.8 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 59.5 kJ/m² Grade Count:2
Charpy Impact Unnotched 1.00 - 11.0 J/cm²4.76 - 52.4 ft-lb/in²Average value: 8.02 J/cm² Grade Count:50
 1.40 - 9.00 J/cm²
@Temperature -40.0 - -30.0 °C
6.66 - 42.8 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 6.65 J/cm² Grade Count:16
Charpy Impact, Notched 0.200 - 9.00 J/cm²0.952 - 42.8 ft-lb/in²Average value: 1.49 J/cm² Grade Count:60
 0.800 - 7.00 J/cm²
@Temperature -40.0 - -30.0 °C
3.81 - 33.3 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 1.77 J/cm² Grade Count:18
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+11 - 1.00e+17 ohm-cm1.00e+11 - 1.00e+17 ohm-cmAverage value: 5.57e+15 ohm-cm Grade Count:30
Surface Resistance 1.00e+12 - 8.10e+16 ohm1.00e+12 - 8.10e+16 ohmAverage value: 9.01e+15 ohm Grade Count:16
Dielectric Constant 3.70 - 6.103.70 - 6.10Average value: 4.53 Grade Count:18
Dielectric Strength 16.0 - 43.0 kV/mm406 - 1090 kV/inAverage value: 27.5 kV/mm Grade Count:22
Dissipation Factor 0.00400 - 0.05000.00400 - 0.0500Average value: 0.0169 Grade Count:16
Arc Resistance 145 - 300 sec145 - 300 secAverage value: 223 sec Grade Count:4
Comparative Tracking Index 325 - 600 V325 - 600 VAverage value: 556 V Grade Count:32
Hot Wire Ignition, HWI 120 - 150 sec120 - 150 secAverage value: 140 sec Grade Count:3
High Amp Arc Ignition, HAI 60.0 - 119 arcs60.0 - 119 arcsAverage value: 77.5 arcs Grade Count:3
High Voltage Arc-Tracking Rate, HVTR 4.00 - 16.0 mm/min0.157 - 0.630 in/minAverage value: 11.0 mm/min Grade Count:3
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 - 50.0 µm/m-°C6.67 - 27.8 µin/in-°FAverage value: 22.0 µm/m-°C Grade Count:29
 6.00 - 35.0 µm/m-°C
@Temperature -40.0 - 249 °C
3.33 - 19.4 µin/in-°F
@Temperature -40.0 - 480 °F
Average value: 12.7 µm/m-°C Grade Count:10
CTE, linear, Transverse to Flow 40.0 - 66.0 µm/m-°C22.2 - 36.7 µin/in-°FAverage value: 53.4 µm/m-°C Grade Count:17
 46.0 - 150 µm/m-°C
@Temperature -40.0 - 249 °C
25.6 - 83.3 µin/in-°F
@Temperature -40.0 - 480 °F
Average value: 83.9 µm/m-°C Grade Count:12
Thermal Conductivity 0.350 - 1.20 W/m-K2.43 - 8.33 BTU-in/hr-ft²-°FAverage value: 0.633 W/m-K Grade Count:3
 0.240 - 0.240 W/m-K
@Temperature 325 - 325 °C
1.67 - 1.67 BTU-in/hr-ft²-°F
@Temperature 617 - 617 °F
Average value: 0.240 W/m-K Grade Count:1
Melting Point 260 - 335 °C500 - 635 °FAverage value: 313 °C Grade Count:54
Maximum Service Temperature, Air 120 - 270 °C248 - 518 °FAverage value: 184 °C Grade Count:15
Deflection Temperature at 0.46 MPa (66 psi) 120 - 310 °C248 - 590 °FAverage value: 276 °C Grade Count:26
Deflection Temperature at 1.8 MPa (264 psi) 90.0 - 320 °C194 - 608 °FAverage value: 275 °C Grade Count:80
Deflection Temperature at 8.0 MPa 105 - 250 °C221 - 482 °FAverage value: 208 °C Grade Count:11
Vicat Softening Point 100 - 313 °C212 - 595 °FAverage value: 258 °C Grade Count:9
Glass Transition Temp, Tg 45.0 - 144 °C113 - 291 °FAverage value: 93.7 °C Grade Count:12
UL RTI, Electrical 85.0 - 140 °C185 - 284 °FAverage value: 134 °C Grade Count:3
Flammability, UL94 HB - V-0HB - V-0Grade Count:42
Flame Spread 25.0 - 80.0 mm/min0.984 - 3.15 in/minAverage value: 44.5 mm/min Grade Count:4
Oxygen Index 23.0 - 27.0 %23.0 - 27.0 %Average value: 25.3 % Grade Count:4
Glow Wire Test 700 - 960 °C1290 - 1760 °FAverage value: 849 °C Grade Count:4
 
Processing PropertiesMetricEnglishComments
Processing Temperature 296 - 345 °C565 - 653 °FAverage value: 324 °C Grade Count:3
Nozzle Temperature 320 - 345 °C608 - 653 °FAverage value: 331 °C Grade Count:8
Melt Temperature 270 - 360 °C518 - 680 °FAverage value: 323 °C Grade Count:68
Mold Temperature 65.6 - 180 °C150 - 356 °FAverage value: 130 °C Grade Count:59
Drying Temperature 80.0 - 130 °C176 - 266 °FAverage value: 111 °C Grade Count:56
Moisture Content 0.0300 - 0.200 %0.0300 - 0.200 %Average value: 0.0708 % Grade Count:48
Dew Point -31.7 - -28.9 °C-25.0 - -20.0 °FAverage value: -30.1 °C Grade Count:7
Injection Pressure 41.4 - 124 MPa6000 - 18000 psiAverage value: 88.2 MPa Grade Count:9

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyphthalamide (PPA)
Overview of materials for Polyphthalamide (PPA), 30% Glass Fiber Reinforced
Overview of materials for Polyphthalamide (PPA), 40% Glass Fiber Reinforced
Overview of materials for Polyphthalamide (PPA), 10% Glass Fiber Reinforced
Overview of materials for Polyphthalamide (PPA), 20% Glass Fiber Reinforced

O4615 / 78363

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.