MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LATI Laramid G/60 PPA, 60% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA)

Material Notes: Semi-aromatic polyamide (PPA) based compound. Glass fibers. Very good thermal properties. Good chemical resistance. Low moisture absorption.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Information provided by Lati Industria Termoplastici S.p.A.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.78 g/cc
Linear Mold Shrinkage, Flow 0.0015 - 0.0035 cm/cm
Linear Mold Shrinkage, Transverse 0.0040 - 0.0065 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 100 MPa
@Temperature 150 °C
 165 MPa
@Temperature 120 °C
 215 MPa
@Temperature 90.0 °C
 240 MPa
@Temperature 60.0 °C
 280 MPa
@Temperature 23.0 °C
Elongation at Break 1.8 %
@Temperature 23.0 °C
 1.9 %
@Temperature 60.0 °C
 2.2 %
@Temperature 90.0 °C
 3.3 %
@Temperature 120 °C
 5.0 %
@Temperature 150 °C
Tensile Modulus 6500 MPa
@Temperature 150 °C
 15000 MPa
@Temperature 120 °C
 20000 MPa
@Temperature 90.0 °C
 22000 MPa
@Temperature 60.0 °C
 24000 MPa
@Temperature 23.0 °C
Charpy Impact Unnotched 90.0 kJ/m²
Charpy Impact, Notched 15.0 kJ/m²
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 150 °C
Deflection Temperature at 0.46 MPa (66 psi) 290 °C
Deflection Temperature at 1.8 MPa (264 psi) 280 °C
Vicat Softening Point 280 °C
@Load 5.00 kg
Flammability, UL94 HB
@Thickness 3.00 mm
 HB
@Thickness 1.50 mm
 HB
@Thickness 0.750 mm
Oxygen Index 42 %
Glow Wire Test 750 °C
@Thickness 1.00 mm
GWFI/GWT
 750 °C
@Thickness 2.00 mm
GWFI/GWT
 
Processing PropertiesOriginal ValueComments
Melt Temperature 310 - 340 °C
Mold Temperature 150 - 170 °C
Drying Temperature 120 - 130 °C
@Time 10800 sec
 
Descriptive Properties
ISO Shrinkage - Pressure60 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LATI Latigloss 57 G/60 F2 PPA, 60% Glass Fiber Reinforced
LATI Laramid G/15 PPA, 15% Glass Fiber Reinforced
Overview of materials for Polyphthalamide (PPA)
Lehvoss LUVOCOM® 20-7094 Polyphthalamide with carbon fiber and PTFE
Evonik Trogamid® T-GF35 35% Glass Reinforced Amorphous Nylon

PLATH9626 / 177322

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.