MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LATI Latigloss 57 G/60 F2 PPA, 60% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA)

Material Notes: Product with high mechanical properties and exceptional surface finish based on Semi-aromatic polyamide (PPA). Glass fibers. Potentially suitable for food/medical contact application.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Information provided by Lati Industria Termoplastici S.p.A.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.77 g/cc0.0639 lb/in³
Linear Mold Shrinkage, Flow 0.0015 - 0.0025 cm/cm0.0015 - 0.0025 in/in
Linear Mold Shrinkage, Transverse 0.0025 - 0.0045 cm/cm0.0025 - 0.0045 in/in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break  70.0 MPa
@Temperature 150 °C
10200 psi
@Temperature 302 °F
 130 MPa
@Temperature 120 °C
18900 psi
@Temperature 248 °F
 210 MPa
@Temperature 90.0 °C
30500 psi
@Temperature 194 °F
 250 MPa
@Temperature 60.0 °C
36300 psi
@Temperature 140 °F
 290 MPa
@Temperature 23.0 °C
42100 psi
@Temperature 73.4 °F
Elongation at Break  1.6 %
@Temperature 23.0 °C
1.6 %
@Temperature 73.4 °F
 1.7 %
@Temperature 60.0 °C
1.7 %
@Temperature 140 °F
 1.9 %
@Temperature 90.0 °C
1.9 %
@Temperature 194 °F
 3.0 %
@Temperature 120 °C
3.0 %
@Temperature 248 °F
 4.5 %
@Temperature 150 °C
4.5 %
@Temperature 302 °F
Tensile Modulus  6.00 GPa
@Temperature 150 °C
870 ksi
@Temperature 302 °F
 15.5 GPa
@Temperature 120 °C
2250 ksi
@Temperature 248 °F
 21.5 GPa
@Temperature 90.0 °C
3120 ksi
@Temperature 194 °F
 23.5 GPa
@Temperature 60.0 °C
3410 ksi
@Temperature 140 °F
 25.0 GPa
@Temperature 23.0 °C
3630 ksi
@Temperature 73.4 °F
Charpy Impact Unnotched 7.50 J/cm²35.7 ft-lb/in²
Charpy Impact, Notched 1.00 J/cm²4.76 ft-lb/in²
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 150 °C302 °F
Deflection Temperature at 0.46 MPa (66 psi) 285 °C545 °F
Deflection Temperature at 1.8 MPa (264 psi) 260 °C500 °F
Vicat Softening Point 260 °C
@Load 5.00 kg
500 °F
@Load 11.0 lb
 
Processing PropertiesMetricEnglishComments
Melt Temperature 310 - 340 °C590 - 644 °F
Mold Temperature 150 - 170 °C302 - 338 °F
Drying Temperature 120 - 130 °C
@Time 10800 sec
248 - 266 °F
@Time 3.00 hour
 
Descriptive Properties
ISO Shrinkage - Pressure60 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LATI Laramid G/60 PPA, 60% Glass Fiber Reinforced
LATI Laramid K/40 HM PPA, 40% Carbon Fiber Reinforced
RTP Company VLF 84009 Polyphthalamide (PPA), Long Glass Fiber - Heat Stabilized
RTP Company RTP 4009 Polyphthalamide (PPA), Glass Fiber
PlastiComp Complet® LCF40 - PP Homopolymer Polypropylene, 40% Long Carbon Fiber Reinforced

PLATH9821 / 177517

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.