MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LG Chemical KEYFLEX TO1192A Olefin Type TPE
Categories: Polymer; Thermoplastic; Elastomer, TPE; Olefinic TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Description: Injection Molding, TPV, General Purpose, Soft Touch

Application: Automotive Interior

CAS: 9003-07-0, 9010-79-1, 64742-54-7, 1333-86-4 and 9002-88-4

Information provided by LG Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.930 g/cc0.930 g/ccASTM D792
Melt Flow 20 g/10 min
@Load 10.0 kg,
Temperature 230 °C
20 g/10 min
@Load 22.0 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D <= 92<= 92ASTM D2240
Elongation at Break 700 %
@Thickness 2.00 mm
700 %
@Thickness 0.0787 in
50mm/min; ASTM D638
Izod Impact, Notched  NB
@Thickness 6.40 mm,
Temperature 23.0 °C
NB
@Thickness 0.252 in,
Temperature 73.4 °F
ASTM D256
 NB
@Thickness 6.40 mm,
Temperature -40.0 °C
NB
@Thickness 0.252 in,
Temperature -40.0 °F
ASTM D256
Tear Strength 53.9 kN/m308 pli50mm/min, @ Break; ASTM D624
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 180 - 200 °C356 - 392 °FInjection Molding
Middle Barrel Temperature 180 - 220 °C356 - 428 °FInjection Molding
Front Barrel Temperature 200 - 230 °C392 - 446 °FInjection Molding
Nozzle Temperature 200 - 240 °C392 - 464 °FInjection Molding
Melt Temperature 200 - 240 °C392 - 464 °FInjection Molding
Mold Temperature 40.0 - 60.0 °C104 - 140 °FInjection Molding
Drying Temperature 60.0 - 90.0 °C140 - 194 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
Back Pressure 29.4 - 58.8 MPa4260 - 8530 psiInjection Molding
Screw Speed 30 - 60 rpm30 - 60 rpmInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow INFUSE™ 9817 Olefin Block Copolymer
A. Schulman POLYTROPE™ TPP 530 Injection Molding Grade Olefinic Thermoplastic Elastomer
LG Chemical KEYFLEX TO1088AV Olefin Type TPE
A. Schulman POLYTROPE™ TPP 620 Olefinic Elastomer
Avient Elastamax™ XL-2055 Thermoplastic Polyolefin Elastomer (TPO (POE))

PLAY450 / 148460

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.