MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ASTM A526 Galvanized Steel
Categories: Metal; Ferrous Metal; ASTM Steel; Carbon Steel; Low Carbon Steel

Material Notes: Lock-forming quality zinc coated (galvanized) steel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/ccTypical of ASTM Steel
Coating Weight 61.0 g/m²alloyed coating A 25; single-spot test, both sides
 61.0 g/m²regular coating G 30; single-spot test, both sides
 76.0 g/m²alloyed coating A 25; triple-spot test, both sides
 91.0 g/m²alloyed coating A 40; single-spot test, both sides
 91.0 g/m²regular coating G 30; triple-spot test, both sides
 122 g/m²alloyed coating A 40; triple-spot test, both sides
 152 g/m²alloyed coating A 60; single-spot test, both sides
 152 g/m²regular coating G 60; single-spot test, both sides
 183 g/m²regular coating G 60; triple-spot test, both sides
 183 g/m²alloyed coating A 60; triple-spot test, both sides
 244 g/m²regular coating G 90; single-spot test, both sides
 275 g/m²regular coating G 90; triple-spot test, both sides
 305 g/m²regular coating G 115; single-spot test, both sides
 351 g/m²regular coating G 115; triple-spot test, both sides
 366 g/m²regular coating G 140; single-spot test, both sides
 427 g/m²regular coating G 165; single-spot test, both sides
 427 g/m²regular coating G 140; triple-spot test, both sides
 488 g/m²regular coating G 185; single-spot test, both sides
 503 g/m²regular coating G 165; triple-spot test, both sides
 549 g/m²regular coating G 210; single-spot test, both sides
 564 g/m²regular coating G 185; triple-spot test, both sides
 610 g/m²regular coating G 235; single-spot test, both sides
 640 g/m²regular coating G 210; triple-spot test, both sides
 717 g/m²regular coating G 235; triple-spot test, both sides
 
Mechanical PropertiesOriginal ValueComments
Modulus of Elasticity 200 GPaTypical Carbon Steel
Bulk Modulus 160 GPaTypical for Steel
Poissons Ratio 0.29Typical Carbon Steel
Shear Modulus 80.0 GPaTypical for Steel
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000170 ohm-cmTypical Carbon Steel
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.0 µm/m-°CTypical Carbon Steel
Specific Heat Capacity 0.470 J/g-°CTypical Carbon Steel
Thermal Conductivity 52.0 W/m-KTypical Carbon Steel
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.15 %
Copper, Cu <= 0.20 %
Iron, Fe 99.4875 %as balance
Manganese, Mn <= 0.60 %
Phosphorus, P <= 0.035 %
Sulfur, S <= 0.040 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ASTM A642 Galvanized Steel
ASTM A525 Galvanized Steel
ASTM A528 Galvanized Steel
JIS S45C Steel, Normalized
ASTM A36 Steel, plate

MSA526 / 142784

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.