MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Morgan Advanced Ceramics Firecrete 4X Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: Chamotte Corundum raw material base. Hydraulic bond. A high alumina, general purpose castables for service temperature to 1650°/3000°F. Used for casting burner blocks, door lining, car tops, crucible furnace linings and special shapes. High purity for performance in special furnace atmospheres.

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramics
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 2.21 g/cc0.0798 lb/in³dried to 110°C
Grain Size <= 5000 µm<= 5000 µm
 
Mechanical PropertiesMetricEnglishComments
Compressive Strength 24.5 MPa3550 psiCold Crushing Strength, MST
 29.4 MPa
@Treatment Temp. 1000 °C
4260 psi
@Treatment Temp. 1830 °F
Cold Crushing Strength
 34.2 MPa
@Treatment Temp. 815 °C
4960 psi
@Treatment Temp. 1500 °F
Cold Crushing Strength
 39.2 MPa
@Treatment Temp. 110 °C
5690 psi
@Treatment Temp. 230 °F
Cold Crushing Strength
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity  1.02 W/m-K
@Temperature 400 °C
7.08 BTU-in/hr-ft²-°F
@Temperature 752 °F
 1.07 W/m-K
@Temperature 600 °C
7.43 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 1.14 W/m-K
@Temperature 800 °C
7.91 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 1.28 W/m-K
@Temperature 1000 °C
8.88 BTU-in/hr-ft²-°F
@Temperature 1830 °F
 1.58 W/m-K
@Temperature 1200 °C
11.0 BTU-in/hr-ft²-°F
@Temperature 2190 °F
Maximum Service Temperature, Air <= 1650 °C<= 3000 °F
Shrinkage 0.20 %0.20 %MST
 0.20 %
@Treatment Temp. 815 °C
0.20 %
@Treatment Temp. 1500 °F
 
Component Elements PropertiesMetricEnglishComments
Al2O3 60 %60 %
CaO 3.7 %3.7 %
Fe2O3 1.0 %1.0 %
K2O+Na2O 0.55 %0.55 %Na2O+ K2O
SiO2 33.1 %33.1 %
TiO2 1.1 %1.1 %
 
Descriptive Properties
Net Material Required (kg/m³)2160
Water Addition11% by weight, 25 kg bag weight

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Kalrez® 6375 FFKM Perfluoroelastomer
DuPont Mobility and Materials Kalrez® 4079 FFKM Perfluoroelastomer
DuPont Mobility and Materials Kalrez® AeroSeal™ 7777 Fluoroelastomer
Precision Polymer Engineering V75C Fluoroelastomer Compound
Precision Polymer Engineering V60V Fluoroelastomer Compound

CMORF6254 / 203038

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.