MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

LG Chemical Lupox® PBT-GP-2306FA 30% GFR Flame Retardant, UV Stabilized PBT  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Glass Fiber Filled, Flame Retardant

Material Notes: Information provided by US distributor Polymer Technology and Services, LLC (PTS).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.34 g/cc0.0484 lb/in³ASTM D792
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 124.1 MPa
@Thickness 3.17 mm
18000 psi
@Thickness 0.125 in
ASTM D638
Tensile Strength, Yield 70.3 MPa10200 psiASTM D638
Elongation at Break 7.0 %7.0 %ASTM D638
Flexural Yield Strength 70.3 MPa10200 psiASTM D570
Flexural Modulus 1.86 GPa270 ksiASTM D570
Izod Impact, Notched 4.27 J/cm8.00 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 220 °C428 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 98.0 °C208 °FASTM D648
Flammability, UL94 V-0
@Thickness 0.7937 mm
V-0
@Thickness 0.03125 in
UL94
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 230 - 245 °C446 - 473 °F
Middle Barrel Temperature 235 - 250 °C455 - 482 °F
Front Barrel Temperature 240 - 250 °C464 - 482 °F
Nozzle Temperature 240 - 260 °C464 - 500 °F
Melt Temperature 240 - 260 °C464 - 500 °F
Mold Temperature 50.0 - 100 °C122 - 212 °FSurface
Drying Temperature 120 °C248 °F5 hr.
 140 °C284 °F3 hr.
 120 °C
@Time 18000 sec
248 °F
@Time 5.00 hour
 140 °C
@Time 10800 sec
284 °F
@Time 3.00 hour
Back Pressure 0.172 - 0.345 MPa25.0 - 50.0 psi
Shot Size 40 - 80 %40 - 80 %
Vent Depth 0.00254 - 0.00381 cm0.00100 - 0.00150 in
 
Descriptive Properties
Ram Speed SettingMedium to Fast
Screw SpeedMedium

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LG Chemical LUPOY GN-2151F Halogen Free Modified PC, 15% Glass Fiber Reinforced, Flame Retardant, Green
BASF Ultradur® B 4406 G6 30% Glass Filled PBT
LG Chemical Lupox® GP2306FY PBT+GF30%
Kingfa PBT-RG301 Flame Retardant, 30% Glass Fiber Reinforced PBT
BASF Ultradur® B 4406 G6 Q113 30% Glass Filled PBT

PLBA07 / 50364

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.