MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay CYCOM® 381 Epoxy Prepreg with IM7 Uni-graphite and 148FAW Epoxy
Categories: Polymer; Thermoset; Carbon Fiber/Thermoset Composite; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes: CYCOM 381 IM7 uni-graphite 148FAW epoxy

CYCOM® 381 epoxy prepreg is an epoxy prepreg that offers a 250°F (121°C) curing system with high 180°F (82°C)/wet mechanical properties yet has the excellent fatigue and durability necessary for primary structure applications.

Features & Benefits:

  • Excellent 180°F (82°C)/wet properties
  • Service temperature to 220°F (104°C)
  • Three- to four-fold increases in fatigue life compared to perhaps all conventional 250°F (121°C) curing epoxy prepregs. This increase is the result of a 10 – 15% higher strain endurance limit.
  • Inherent toughness provides good durability and compression after impact performance
  • Low moisture absorption
  • Excellent for vacuum pressure/oven processing
Applications:
  • Primary and secondary structural aircraft parts requiring 180°F (82°C)/wet retention of properties and/or excellent fatigue behavior
  • Components that require good durability and/or low processing temperatures
  • Helicopter rotor blades
  • Rotating or cycled components
  • Co-cured aluminum assemblies/parts
  • Doublers
  • Propellers
  • Composite repair

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 94800 psiLaminate
 5400 psi
@Temperature 82.0 °C
90°, dry; SACMA SRM-4
 5500 psi
@Temperature 22.0 °C
90°, dry; SACMA SRM-4
 6300 psi
@Temperature -54.0 °C
90°, dry; SACMA SRM-4
 331000 psi
@Temperature 71.0 °C
0°, wet; SACMA SRM-4
 339000 psi
@Temperature 82.0 °C
0°, dry; SACMA SRM-4
 345000 psi
@Temperature 104 °C
0°, dry; SACMA SRM-4
 358000 psi
@Temperature 22.0 °C
0°, dry; SACMA SRM-4
 368000 psi
@Temperature -54.0 °C
0°, dry; SACMA SRM-4
Tensile Modulus 7.72 GPa
@Temperature 82.0 °C
90°, dry; SACMA SRM-4
 8.83 GPa
@Temperature 22.0 °C
90°, dry; SACMA SRM-4
 9.65 GPa
@Temperature -54.0 °C
90°, dry; SACMA SRM-4
 160 GPa
@Temperature 104 °C
0°, dry; SACMA SRM-4
 165 GPa
@Temperature 22.0 °C
0°, dry; SACMA SRM-4
 165 GPa
@Temperature 82.0 °C
0°, dry; SACMA SRM-4
 168 GPa
@Temperature -54.0 °C
0°, dry; SACMA SRM-4
 169 GPa
@Temperature 71.0 °C
0°, wet; SACMA SRM-4
Flexural Strength 180000 psi
@Temperature 104 °C
0°, dry, 3-point
 211000 psi
@Temperature 22.0 °C
0°, dry, 3-point
Flexural Modulus 136 GPa
@Temperature 22.0 °C
0°, dry, 3-point; ASTM D790
 148 GPa
@Temperature 104 °C
0°, dry, 3-point; ASTM D790
Compressive Strength 1296 MPa
@Temperature 71.0 °C
0°, wet; SACMA SRM-1
 1317 MPa
@Temperature 104 °C
0°, dry; SACMA SRM-1
 1393 MPa
@Temperature -54.0 °C
0°, dry; SACMA SRM-1
 1427 MPa
@Temperature 82.0 °C
0°, dry; SACMA SRM-1
 1482 MPa
@Temperature 22.0 °C
0°, dry; SACMA SRM-1
Compressive Modulus 47600 MPa
@Temperature -54.0 °C
0°, dry; SACMA SRM-1
 148000 MPa
@Temperature -54.0 °C
0°, dry; SACMA SRM-1
 148000 MPa
@Temperature 22.0 °C
0°, dry; SACMA SRM-1
 150000 MPa
@Temperature 71.0 °C
0°, wet; SACMA SRM-1
 150000 MPa
@Temperature 82.0 °C
0°, dry; SACMA SRM-1
Shear Modulus 1.90 GPa
@Temperature 104 °C
In-plane, SACMA SRM-7, wet
 3.20 GPa
@Temperature 82.0 °C
In-plane, SACMA SRM-7, wet
 3.40 GPa
@Temperature 121 °C
In-plane, SACMA SRM-7, dry
 3.60 GPa
@Temperature 71.0 °C
In-plane, SACMA SRM-7, wet
 3.80 GPa
@Temperature 82.0 °C
In-plane, SACMA SRM-7, dry
 4.30 GPa
@Temperature 22.0 °C
In-plane, SACMA SRM-7, dry
 5.10 GPa
@Temperature -54.0 °C
In-plane, SACMA SRM-7, dry
Shear Strength 7800 psi
@Temperature 71.0 °C
0° Short Beam, wet; SACMA SRM-8
 7800 psi
@Temperature 71.0 °C
0° Short Beam, Water, 160°F (71°C)/14 days; SACMA SRM-8
 9600 psi
@Temperature 82.0 °C
0° Short Beam, dry; SACMA SRM-8
 10000 psi
@Temperature 104 °C
In-plane, wet; SACMA SRM-7
 11900 psi
@Temperature 82.0 °C
In-plane, wet; SACMA SRM-7
 12800 psi
@Temperature 22.0 °C
0° Short Beam, Fuel, Mil-T-5624, 75°F (24°C)/90 days; SACMA SRM-8
 12900 psi
@Temperature 22.0 °C
0° Short Beam, Cleaning, Mil-C-87936, 75°F (24°C)/7 days; SACMA SRM-8
 13000 psi
@Temperature 22.0 °C
0° Short Beam, MEK, 75°F (24°C)/7 days; ASTM D740
 13200 psi
@Temperature 22.0 °C
0° Short Beam, Hydraulic, Mil-H-83282, 160°F (71°C)/90 days; SACMA SRM-8
 13300 psi
@Temperature 22.0 °C
0° Short Beam, dry; SACMA SRM-8
 13300 psi
@Temperature 22.0 °C
0° Short Beam; SACMA SRM-8
 13500 psi
@Temperature 22.0 °C
0° Short Beam, Deicer, Mil-A-8243, 32°F (0°C)/30 days; SACMA SRM-8
 13600 psi
@Temperature 22.0 °C
0° Short Beam, Oil, Mil-L-7808, 160°F (71°C)/90 days; SACMA SRM-8
 13700 psi
@Temperature 22.0 °C
0° Short Beam, Hydraulic, Mil-H-5606, 160°F (71°C)/90 days; SACMA SRM-8
 13900 psi
@Temperature 71.0 °C
In-plane, wet; SACMA SRM-7
 14000 psi
@Temperature 22.0 °C
0° Short Beam, Oil, Mil-L-23699, 160°F (71°C)/90 days; SACMA SRM-8
 14300 psi
@Temperature 121 °C
In-plane, dry; SACMA SRM-7
 15500 psi
@Temperature 82.0 °C
In-plane, dry; SACMA SRM-7
 15800 psi
@Temperature -54.0 °C
0° Short Beam, dry; SACMA SRM-8
 18600 psi
@Temperature 22.0 °C
In-plane, dry; SACMA SRM-7
 19100 psi
@Temperature -54.0 °C
In-plane, dry; SACMA SRM-7
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 220 °F
 
Processing PropertiesOriginal ValueComments
Gel Time 5.00 - 8.00 min
@Temperature 121 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay CYCOM® 381 Epoxy Prepreg with AS4 Graphite Fabric and 195FAW Epoxy
Solvay CYCOM® 5250-4 BMI Prepreg System with IM7-6K-5HS Woven Carbon Fiber
Hexcel® HexPly® M47 140°C Curing Epoxy Matrix, Woven Carbon Prepreg
APCM DA 4518U Unidirectional Carbon Epoxy Prepreg System
Solvay CYCOM® 5250-4 BMI Prepreg System with IM-7 Carbon Fiber

PCYTED078_1 / 192654

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.