MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Covestro Baytec® MS-051 Polyurethane
Categories: Polymer; Thermoset; Polyurethane, TS

Material Notes: Characterization: Baytec MS-051 is a modified diphenylmethane diisocyanate (MDI)-terminated polyester prepolymer.

Properties / Applications: Baytec MS-051 is a modified diphenylmethane diisocyanate (MDI)-terminated polyester prepolymer used in the manufacture of high-property solid cast polyurethane elastomers. The excellent resilience and low compression-set properties have enabled this material to be used for low-durometer wheels, printing rolls, and squeegee blades. As with any product, use of Baytec MS-051 prepolymer in a given application must be tested (including field testing, etc.) in advance by the user to determine suitability.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity  1.17 g/cc
@Temperature 100 °C
1.17 g/cc
@Temperature 212 °F
 1.18 g/cc
@Temperature 80.0 °C
1.18 g/cc
@Temperature 176 °F
Viscosity  700 cP
@Temperature 100 °C
700 cP
@Temperature 212 °F
 2700 cP
@Temperature 80.0 °C
2700 cP
@Temperature 176 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8080BDO; ASTM D2240
 9393HQEE; ASTM D2240
Tensile Strength at Break 26.3 MPa3810 psiHQEE; ASTM D412
 37.0 MPa5370 psiBDO; ASTM D412
 4.41 MPa
@Thickness 2540 mm
640 psi
@Thickness 100 in
BDO; ASTM D412
 6.00 MPa
@Thickness 5080 mm
870 psi
@Thickness 200 in
BDO; ASTM D412
 8.07 MPa
@Thickness 2540 mm
1170 psi
@Thickness 100 in
HQEE; ASTM D412
 8.14 MPa
@Thickness 7620 mm
1180 psi
@Thickness 300 in
BDO; ASTM D412
 9.89 MPa
@Thickness 5080 mm
1430 psi
@Thickness 200 in
HQEE; ASTM D412
 11.8 MPa
@Thickness 7620 mm
1710 psi
@Thickness 300 in
HQEE; ASTM D412
Elongation at Break 525 %525 %BDO; ASTM D412
 650 %650 %HQEE; ASTM D412
Compressive Strength  0.241 MPa
@Strain 2 %
35.0 psi
@Strain 2 %
BDO; ASTM D575
 0.621 MPa
@Strain 2 %
90.1 psi
@Strain 2 %
HQEE; ASTM D575
 0.724 MPa
@Strain 5.0 %
105 psi
@Strain 5.0 %
BDO; ASTM D575
 1.52 MPa
@Strain 10 %
220 psi
@Strain 10 %
BDO; ASTM D575
 1.69 MPa
@Strain 5.0 %
245 psi
@Strain 5.0 %
HQEE; ASTM D575
 2.28 MPa
@Strain 15 %
331 psi
@Strain 15 %
BDO; ASTM D575
 2.90 MPa
@Strain 10 %
421 psi
@Strain 10 %
HQEE; ASTM D575
 3.07 MPa
@Strain 20 %
445 psi
@Strain 20 %
BDO; ASTM D575
 3.93 MPa
@Strain 25 %
570 psi
@Strain 25 %
BDO; ASTM D575
 3.96 MPa
@Strain 15 %
574 psi
@Strain 15 %
HQEE; ASTM D575
 5.03 MPa
@Strain 20 %
730 psi
@Strain 20 %
HQEE; ASTM D575
 6.21 MPa
@Strain 25 %
901 psi
@Strain 25 %
HQEE; ASTM D575
 10.9 MPa
@Strain 50 %
1580 psi
@Strain 50 %
BDO; ASTM D575
 18.4 MPa
@Strain 50 %
2670 psi
@Strain 50 %
HQEE; ASTM D575
Resilience 5252Bayshore, BDO; ASTM D2632
 5454Bayshore, HQEE; ASTM D2632
Tear Strength 18.4 kN/m105 pliSplit, BDO; ASTM D1938
 49.1 kN/m280 pliSplit, HQEE; ASTM D1938
 66.6 kN/m380 pliDie C, BDO; ASTM D624
 108 kN/m615 pliDie C, HQEE; ASTM D624
Taber Abrasion, mg/1000 Cycles  16
@Load 1.00 kg
16
@Load 2.20 lb
H-18, BDO; ASTM D4060
 34
@Load 1.00 kg
34
@Load 2.20 lb
H-18, HQEE; ASTM D4060
Compression Set  19 %
@Temperature 70.0 °C,
Time 79200 sec
19 %
@Temperature 158 °F,
Time 22.0 hour
HQEE; ASTM D395-B
 24 %
@Temperature 70.0 °C,
Time 79200 sec
24 %
@Temperature 158 °F,
Time 22.0 hour
BDO; ASTM D395-B
 
Thermal PropertiesMetricEnglishComments
Flash Point >= 93.0 °C>= 199 °F
 
Processing PropertiesMetricEnglishComments
Mold Temperature 100 - 110 °C212 - 230 °F
 
Descriptive Properties
AppearanceLight amber liquid
Content4.9-5.2%NCO

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Sorbothane Polyurethane Damping Material, 50 Durometer
Daikin DAI-EL® G-101 Fluoroelastomer Plasticizer with DAI-EL® G-701 Fluoroelastomer
SMAC SMACTANE® SP Damping Material
SMAC SMACTANE® 50 1114S- N03 Damping Material
Shin-Etsu Silicones SF-11500U Fluorosilicone Elastomer

PCOVEST0253 / 202036

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.