MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

General Plastics LAST-A-FOAM® FR-4510 High Density, Rigid Foam
Categories: Other Engineering Material

Material Notes: Product Description: LAST-A-FOAM® high-density, rigid foam products are cost-effective, versatile, strong and durable. They are manufactured using our unique chemical formulas to be exceptionally uniform and consistent in all physical properties. The FR-4500 is a grain-free, machineable tooling board for styling and design models, master models, masters for composite and layup tools, and for mold and foundry patterns. The material also serves as an excellent wood alternative for outdoor signage and display manufacturing. Available in densities from 10 to 50 lbs. per cubic foot.

Key Performance Benefits:

  • Special formulation creates shavings when material is machined, causing less dust
  • Excellent consistency and uniformity throughout entire mass of material
  • Dimensional stability
  • No warp or bow in sheets
  • Large sheets (up to 48” x 96”), thick sheets (up to 22”) available
  • Custom sizes available
Applications:
  • Design prototypes
  • Appearance or “sight” models
  • Styling models
  • Architectural models
  • Master models
  • Temporary models
  • Trim, jigs, and fixtures
  • Thermoforming tools
  • Prototype foundry patterns
  • Mold patterns
  • Topographical maps
  • Dimensional check-fixtures
  • Molds for low-temperature casting (<200 ºF)
  • Prototype/low-volume Vacuum-forming tools
  • CAD model proofs/NC program proofs
  • Tooling aids
  • Molds for low-temperature curing prepregs (<200 ºF)

Information provided by General Plastics Manufacturing Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.160 g/cc0.00578 lb/in³ASTM D1622
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 1515ASTM D2240
Tensile Strength 1.74 MPa253 psiPerpendicular to Rise; ASTM D1623
 1.75 MPa254 psiASTM D1623
 1.79 MPa260 psiParallel to Rise; ASTM D1623
Flexural Strength 2.40 MPa348 psiASTM D790
 2.59 MPa375 psiRise Parallel to Test Span; ASTM D790 Method 1-A
 2.65 MPa385 psiRise Parallel to Beam Thick.; ASTM D790 Method 1-A
Flexural Modulus 0.083344 GPa12.088 ksiASTM D790
 0.10813 GPa15.683 ksiRise Parallel to Beam Thick.; ASTM D790 Method 1-A
 0.11486 GPa16.659 ksiRise Parallel to Test Span; ASTM D790 Method 1-A
Compressive Strength 1.99 MPa289 psiASTM D1621
 1.51 MPa
@Temperature 71.1 °C
219 psi
@Temperature 160 °F
Perpendicular to Rise; ASTM D1621
 1.56 MPa
@Temperature 71.1 °C
226 psi
@Temperature 160 °F
Parallel to Rise; ASTM D1621
 2.06 MPa
@Temperature 23.9 °C
299 psi
@Temperature 75.0 °F
Perpendicular to Rise; ASTM D1621
 2.10 MPa
@Temperature 23.9 °C
304 psi
@Temperature 75.0 °F
Parallel to Rise; ASTM D1621
Compressive Modulus 0.070368 GPa10.206 ksiASTM D1621
 0.05151 GPa
@Temperature 71.1 °C
7.471 ksi
@Temperature 160 °F
Perpendicular to Rise; ASTM D1621
 0.05734 GPa
@Temperature 71.1 °C
8.316 ksi
@Temperature 160 °F
Parallel to Rise; ASTM D1621
 0.06146 GPa
@Temperature 23.9 °C
8.914 ksi
@Temperature 75.0 °F
Perpendicular to Rise; ASTM D1621
 0.0645 GPa
@Temperature 23.9 °C
9.35 ksi
@Temperature 75.0 °F
Parallel to Rise; ASTM D1621
Poissons Ratio 0.300.30
Shear Modulus 0.01963 GPa2.847 ksiASTM C273
Shear Strength 1.41 MPa205 psiASTM C273
 
Thermal PropertiesMetricEnglishComments
CTE, linear 522 µm/m-°C
@Temperature -45.6 - 93.3 °C
290 µin/in-°F
@Temperature -50.0 - 200 °F
GP Method
Thermal Conductivity 0.0379 W/m-K0.263 BTU-in/hr-ft²-°FASTM C518
Glass Transition Temp, Tg 103 °C217 °FASTM E1545-05
 
Descriptive Properties
ColorTerracotta
Surface Roughness1494sanded, SJ-201P per JIS B0601-1982
Tumbling Friability (%)5.120 mins at 60 rpm, ASTM C421

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Elektro-Isola G-Etronax EP FR4 Epoxy, Glass Fabric Reinforcement, Light Yellow, Sheets
G-10 Fiberglass Epoxy Laminate Sheet
Overview of materials for Thermoset Polyester Glass Filled BMC
Park Aerospace Nelco® N4000-7 SI® FR-4 Epoxy Laminate and Prepreg
NOVA Chemicals Dylark® 238P20 High Performance Glass Filled Styrenic

PGENR022 / 186808

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.