MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Sarlink® TPE EE-2235N Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Sarlink EE-2235N is a general purpose thermoplastic elastomer designed for automotive applications, including exterior extruded components. Sarlink EE-2235N is a low hardness, high density, filled grade with good UV resistance and has excellent extrudability.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Good Adhesion; Good Processability; Good Surface Finish; High Density; High Specific Gravity; Low Hardness; UV Resistant

Uses: Automotive Applications; Automotive Exterior Trim; Rubber Replacement

RoHS Compliance: RoHS Compliant

Automotive Specifications: CHRYSLER PS-7000

Form: Pellets

Processing Method: Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.17 g/cc0.0423 lb/in³ASTM D792
Melt Flow 0.60 g/10 min
@Load 2.16 kg,
Temperature 230 °C
0.60 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 3838ASTM D2240
 35
@Time 15.0 sec
35
@Time 0.00417 hour
ASTM D2240
Tensile Strength at Break 3.10 MPa450 psiFlow; ASTM D412
 5.24 MPa760 psiAcross Flow; ASTM D412
Tensile Stress at Strain  0.552 MPa
@Strain 100 %
80.0 psi
@Strain 100 %
Across Flow; ASTM D412
 0.896 MPa
@Strain 100 %
130 psi
@Strain 100 %
Flow; ASTM D412
Elongation at Break 730 %730 %Flow; ASTM D412
 930 %930 %Across Flow; ASTM D412
Tear Strength 18.8 kN/m107 pliAcross Flow; ASTM D624
Compression Set  10 %
@Temperature 22.8 °C,
Time 79200 sec
10 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 24 %
@Temperature 70.0 °C,
Time 79200 sec
24 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395
 79 %
@Temperature 125 °C,
Time 252000 sec
79 %
@Temperature 257 °F,
Time 70.0 hour
ASTM D395
 
Processing PropertiesMetricEnglishComments
Zone 1 193 - 204 °C380 - 400 °F
Zone 2 199 - 210 °C390 - 410 °F
Zone 3 204 - 216 °C400 - 420 °F
Zone 5 210 - 221 °C410 - 430 °F
Die Temperature 216 - 227 °C420 - 440 °F
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Sarlink® TPE RV-2235B-01 XRD Thermoplastic Elastomer
Teknor Apex Sarlink® TPE RV-2235B Thermoplastic Elastomer
Teknor Apex Sarlink® TPE ME-2245B Thermoplastic Elastomer

PTEKNQ1025 / 237516

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.