MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Sarlink® TPE RV-2235B Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Sarlink RV-2235B is a high performance thermoplastic used in transportation applications. Sarlink RV-2235B is a low hardness grade and UV resistant. This grade can be processed by extrusion.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Filled; Light Stabilized; Low Hardness; Lubricated; Medium Flow; Slip; Sunlight Resistant; UV Absorbing

Uses: Automotive Applications; Automotive Exterior Parts; Automotive Exterior Trim

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.950 g/cc0.0343 lb/in³ISO 1183
Viscosity 209 cP
@Shear Rate 206 1/s,
Temperature 200 °C
209 cP
@Shear Rate 206 1/s,
Temperature 392 °F
ASTM D3835
Melt Flow 10 g/10 min
@Load 5.00 kg,
Temperature 200 °C
10 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  41
@Time 15.0 sec
41
@Time 0.00417 hour
Injection Molded; ISO 868
 42
@Time 5.00 sec
42
@Time 0.00139 hour
Injection Molded; ISO 868
 44
@Time 1.00 sec
44
@Time 0.000278 hour
Injection Molded; ISO 868
 43.2
@Treatment Temp. 125 °C,
Time 15.0 sec
43.2
@Treatment Temp. 257 °F,
Time 0.00417 hour
Change in Air, 168 hr; ISO 888
 44.1
@Treatment Temp. 110 °C,
Time 15.0 sec
44.1
@Treatment Temp. 230 °F,
Time 0.00417 hour
Change in Air, 1008 hr; ISO 888
 44.3
@Treatment Temp. 125 °C,
Time 5.00 sec
44.3
@Treatment Temp. 257 °F,
Time 0.00139 hour
Change in Air, 168 hr; ISO 888
 45.5
@Treatment Temp. 110 °C,
Time 5.00 sec
45.5
@Treatment Temp. 230 °F,
Time 0.00139 hour
Change in Air, 1008 hr; ISO 888
 46.1
@Treatment Temp. 125 °C,
Time 1.00 sec
46.1
@Treatment Temp. 257 °F,
Time 0.000278 hour
Change in Air, 168 hr; ISO 888
 47.5
@Treatment Temp. 110 °C,
Time 1.00 sec
47.5
@Treatment Temp. 230 °F,
Time 0.000278 hour
Change in Air, 1008 hr; ISO 888
Tensile Strength at Break 2.40 MPa348 psiFlow, Type 1, 20 in/min; ISO 37
 6.20 MPa899 psiAcross Flow, Type 1, 20 in/min; ISO 37
 2.30 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
333 psi
@Treatment Temp. 257 °F,
Time 168 hour
Flow, Type 1, Change in Air; ISO 188
 2.40 MPa
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
348 psi
@Treatment Temp. 230 °F,
Time 1008 hour
Flow, Type 1, Change in Air; ISO 188
 3.60 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
521 psi
@Treatment Temp. 257 °F,
Time 168 hour
Across Flow, Type 1, Change in Air; ISO 188
 8.68 MPa
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
1260 psi
@Treatment Temp. 230 °F,
Time 1008 hour
Across Flow, Type 1, Change in Air; ISO 188
Tensile Stress at Strain  0.731 MPa
@Strain 100 %
106 psi
@Strain 100 %
Across Flow, Type 1, 20 in/min; ISO 37
 1.90 MPa
@Strain 100 %
276 psi
@Strain 100 %
Flow, Type 1, 20 in/min; ISO 37
 0.711 MPa
@Strain 100 %,
Treatment Temp. 125 °C
103 psi
@Strain 100 %,
Treatment Temp. 257 °F
Across Flow, Type 1, Change in Air, 6.61 in; ISO 188
 0.811 MPa
@Strain 100 %,
Treatment Temp. 110 °C
118 psi
@Strain 100 %,
Treatment Temp. 230 °F
Across Flow, Type 1, Change in Air, 1008 hr; ISO 188
 2.00 MPa
@Strain 100 %,
Treatment Temp. 125 °C
291 psi
@Strain 100 %,
Treatment Temp. 257 °F
Flow, Type 1, Change in Air, 168 hr; ISO 188
 2.08 MPa
@Strain 100 %,
Treatment Temp. 110 °C
302 psi
@Strain 100 %,
Treatment Temp. 230 °F
Flow, Type 1, Change in Air, 1008 hr; ISO 188
Elongation at Break 240 %240 %Flow, Type 1, 20 in/min; ISO 37
 870 %870 %Across Flow, Type 1, 20 in/min; ISO 37
 338 %
@Treatment Temp. 125 °C,
Time 605000 sec
338 %
@Treatment Temp. 257 °F,
Time 168 hour
Flow, Type 1, Change in Air; ISO 188
 341 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
341 %
@Treatment Temp. 230 °F,
Time 1008 hour
Flow, Type 1, Change in Air; ISO 188
 952 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
952 %
@Treatment Temp. 230 °F,
Time 1008 hour
Across Flow, Type 1, Change in Air; ISO 188
 1630 %
@Treatment Temp. 125 °C,
Time 605000 sec
1630 %
@Treatment Temp. 257 °F,
Time 168 hour
Across Flow, Type 1, Change in Air; ISO 188
Tear Strength 12.1 kN/m69.0 pliAcross Flow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
 22.8 kN/m130 pliFlow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
Compression Set  11 %
@Temperature 22.8 °C,
Time 79200 sec
11 %
@Temperature 73.0 °F,
Time 22.0 hour
Type 1; ISO 815
 60 %
@Temperature 70.0 °C,
Time 79200 sec
60 %
@Temperature 158 °F,
Time 22.0 hour
Type 1; ISO 815
 71 %
@Temperature 90.0 °C,
Time 252000 sec
71 %
@Temperature 194 °F,
Time 70.0 hour
Type 1; ISO 815
 84 %
@Temperature 125 °C,
Time 252000 sec
84 %
@Temperature 257 °F,
Time 70.0 hour
Type 1; ISO 815
 
Processing PropertiesMetricEnglishComments
Zone 1 182 - 232 °C360 - 450 °F
Zone 2 188 - 238 °C370 - 460 °F
Zone 3 193 - 243 °C380 - 470 °F
Zone 5 199 - 249 °C390 - 480 °F
Die Temperature 199 - 249 °C390 - 480 °F
Screw Speed 30 - 100 rpm30 - 100 rpm
 
Descriptive Properties
AppearanceBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Sarlink® TPE RV-2250D BLK 111 Thermoplastic Elastomer
Teknor Apex Sarlink® TPE RV-2235B-01 XRD Thermoplastic Elastomer
Teknor Apex Sarlink® TPE ME-2245B Thermoplastic Elastomer
Teknor Apex Sarlink® TPE EE-2235N Thermoplastic Elastomer
Radici Raditer® B RV 100 Polybutylene Terephthalate with 10% Glass fiber

PTEKNQ1123 / 237614

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.