422 Stainless Steel 540°C (1000°F) temper
Categories:
Metal
;
Ferrous Metal
;
Stainless Steel
;
T 400 Series Stainless Steel
Material Notes:
austenitized at 1040°C for 1 hour, oil quench, temper for 2 hours
Key Words:
UNS S42200, AMS 5655, ASTM A565, SAE J467, DIN 1.4935, JIS SUH 616
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
7.80
g/cc
0.282
lb/in³
Mechanical Properties
Metric
English
Comments
Tensile Strength, Ultimate
1610
MPa
234000
psi
1165
MPa
@Temperature 540 °C
169000
psi
@Temperature 1000 °F
Tensile Strength, Yield
1005
MPa
@Strain 0.2 %
145800
psi
@Strain 0.2 %
869
MPa
@Strain 0.2 %,
Temperature 540 °C
126000
psi
@Strain 0.2 %,
Temperature 1000 °F
Elongation at Break
16 %
16 %
in 36 mm
16 %
@Temperature 540 °C
16 %
@Temperature 1000 °F
in 36 mm
Tensile Modulus
199.2
GPa
28890
ksi
141.4
GPa
@Temperature 595 °C
20510
ksi
@Temperature 1100 °F
166.6
GPa
@Temperature 425 °C
24160
ksi
@Temperature 797 °F
189.6
GPa
@Temperature 260 °C
27500
ksi
@Temperature 500 °F
Poissons Ratio
0.20
0.20
Calculated
Shear Modulus
62.0
GPa
@Temperature 593 °C
8990
ksi
@Temperature 1100 °F
72.4
GPa
@Temperature 427 °C
10500
ksi
@Temperature 800 °F
79.3
GPa
@Temperature 260 °C
11500
ksi
@Temperature 500 °F
82.7
GPa
@Temperature 23.9 °C
12000
ksi
@Temperature 75.0 °F
Electrical Properties
Metric
English
Comments
Electrical Resistivity
0.0000610
ohm-cm
0.0000610
ohm-cm
Thermal Properties
Metric
English
Comments
CTE, linear
11.2
µm/m-°C
@Temperature 0.000 - 100 °C
6.22
µin/in-°F
@Temperature 32.0 - 212 °F
11.3
µm/m-°C
@Temperature 0.000 - 315 °C
6.28
µin/in-°F
@Temperature 32.0 - 599 °F
11.9
µm/m-°C
@Temperature 0.000 - 540 °C
6.61
µin/in-°F
@Temperature 32.0 - 1000 °F
12.1
µm/m-°C
@Temperature 0.000 - 650 °C
6.72
µin/in-°F
@Temperature 32.0 - 1200 °F
Specific Heat Capacity
0.460
J/g-°C
@Temperature 0.000 - 100 °C
0.110
BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity
23.9
W/m-K
@Temperature 100 °C
166
BTU-in/hr-ft²-°F
@Temperature 212 °F
27.3
W/m-K
@Temperature 500 °C
189
BTU-in/hr-ft²-°F
@Temperature 932 °F
Melting Point
1470
-
1480
°C
2680
-
2700
°F
Solidus
1470
°C
2680
°F
Liquidus
1480
°C
2700
°F
Component Elements Properties
Metric
English
Comments
Carbon, C
0.20 - 0.25 %
0.20 - 0.25 %
Chromium, Cr
12 %
12 %
Iron, Fe
84 %
84 %
Manganese, Mn
<= 1.0 %
<= 1.0 %
Molybdenum, Mo
1.0 %
1.0 %
Nickel, Ni
0.75 %
0.75 %
Phosphorus, P
<= 0.025 %
<= 0.025 %
Silicon, Si
<= 0.75 %
<= 0.75 %
Sulfur, S
<= 0.025 %
<= 0.025 %
Tungsten, W
1.0 %
1.0 %
Vanadium, V
0.23 %
0.23 %
References
for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
AISI Type 410S Stainless Steel, tempered at 540°C (1000°F)
410 Stainless Steel, tempered at 540°C (1000°F)
422 Stainless Steel 650°C (1200°F) temper
422 Stainless Steel 480°C (900°F) temper
422 Stainless Steel 370°C temper
MQ422AK / 13094
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.