MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Schott IRG 23 Infrared Chalcogenide Glass
Categories: Ceramic; Glass; Optical; Sulfide/Chalcogenide

Material Notes: IRG 23 has excellent transmission in the SWIR, MWIR, & LWIR and has the highest refractive index of the IR series glasses. Physical properties such as low dn/dT and low dispersion enable optical engineers to design color corrected optical systems without thermal defocusing. IRG 23 is optimized for pairing within the family of IR glasses and with other IR materials to support cost effective and high performance optical designs. Furthermore, IRG 23 can be processed by conventional grinding and polishing, single point diamond turning, or molding to support low to high volume component level fabrication.

Information provided by SCHOTT.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 4.84 g/cc0.175 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 1.361.36[GPA]
Modulus of Elasticity 22.0 GPa3190 ksi
Poissons Ratio 0.2370.237Calculated
Fracture Toughness 0.414 MPa-m½0.377 ksi-in½
Shear Modulus 8.89 GPa1290 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear 13.4 µm/m-°C7.44 µin/in-°F
Specific Heat Capacity 0.320 J/g-°C0.0765 BTU/lb-°F
Thermal Conductivity 0.220 W/m-K1.53 BTU-in/hr-ft²-°F
Transformation Temperature, Tg 275 °C527 °F
 
Optical PropertiesMetricEnglishComments
Refractive Index  2.781
@Wavelength 12000 nm
2.781
@Wavelength 12000 nm
 2.784
@Wavelength 11000 nm
2.784
@Wavelength 11000 nm
 2.786
@Wavelength 10000 nm
2.786
@Wavelength 10000 nm
 2.789
@Wavelength 9000 nm
2.789
@Wavelength 9000 nm
 2.791
@Wavelength 8000 nm
2.791
@Wavelength 8000 nm
 2.794
@Wavelength 7000 nm
2.794
@Wavelength 7000 nm
 2.796
@Wavelength 6000 nm
2.796
@Wavelength 6000 nm
 2.799
@Wavelength 5000 nm
2.799
@Wavelength 5000 nm
 2.803
@Wavelength 4000 nm
2.803
@Wavelength 4000 nm
 2.811
@Wavelength 3000 nm
2.811
@Wavelength 3000 nm
 2.832
@Wavelength 2000 nm
2.832
@Wavelength 2000 nm
 2.863
@Wavelength 1500 nm
2.863
@Wavelength 1500 nm
 2.908
@Wavelength 1200 nm
2.908
@Wavelength 1200 nm
IR Transmittance  0.00 %
@Wavelength 1100 nm
0.00 %
@Wavelength 1100 nm
 10.28 %
@Wavelength 13000 nm
10.28 %
@Wavelength 13000 nm
 15.54 %
@Wavelength 12500 nm
15.54 %
@Wavelength 12500 nm
 19.58 %
@Wavelength 1200 nm
19.58 %
@Wavelength 1200 nm
 21.22 %
@Wavelength 13500 nm
21.22 %
@Wavelength 13500 nm
 39.09 %
@Wavelength 14000 nm
39.09 %
@Wavelength 14000 nm
 39.11 %
@Wavelength 12000 nm
39.11 %
@Wavelength 12000 nm
 44.77 %
@Wavelength 1300 nm
44.77 %
@Wavelength 1300 nm
 52.98 %
@Wavelength 1400 nm
52.98 %
@Wavelength 1400 nm
 54.56 %
@Wavelength 1450 nm
54.56 %
@Wavelength 1450 nm
 56.04 %
@Wavelength 11500 nm
56.04 %
@Wavelength 11500 nm
 56.45 %
@Wavelength 1550 nm
56.45 %
@Wavelength 1550 nm
 57.15 %
@Wavelength 1650 nm
57.15 %
@Wavelength 1650 nm
 57.7 %
@Wavelength 1750 nm
57.7 %
@Wavelength 1750 nm
 58.05 %
@Wavelength 1850 nm
58.05 %
@Wavelength 1850 nm
 58.48 %
@Wavelength 1950 nm
58.48 %
@Wavelength 1950 nm
 58.69 %
@Wavelength 2050 nm
58.69 %
@Wavelength 2050 nm
 58.92 %
@Wavelength 2150 nm
58.92 %
@Wavelength 2150 nm
 58.94 %
@Wavelength 8000 nm
58.94 %
@Wavelength 8000 nm
 59.04 %
@Wavelength 2250 nm
59.04 %
@Wavelength 2250 nm
 59.16 %
@Wavelength 11000 nm
59.16 %
@Wavelength 11000 nm
 59.22 %
@Wavelength 5000 nm
59.22 %
@Wavelength 5000 nm
 59.28 %
@Wavelength 3000 nm
59.28 %
@Wavelength 3000 nm
 59.3 %
@Wavelength 2350 nm
59.3 %
@Wavelength 2350 nm
 59.47 %
@Wavelength 2450 nm
59.47 %
@Wavelength 2450 nm
 59.55 %
@Wavelength 2500 nm
59.55 %
@Wavelength 2500 nm
 59.97 %
@Wavelength 4500 nm
59.97 %
@Wavelength 4500 nm
 60.27 %
@Wavelength 3500 nm
60.27 %
@Wavelength 3500 nm
 60.6 %
@Wavelength 10500 nm
60.6 %
@Wavelength 10500 nm
 60.76 %
@Wavelength 4000 nm
60.76 %
@Wavelength 4000 nm
 61.19 %
@Wavelength 8500 nm
61.19 %
@Wavelength 8500 nm
 61.56 %
@Wavelength 9000 nm
61.56 %
@Wavelength 9000 nm
 61.62 %
@Wavelength 9500 nm
61.62 %
@Wavelength 9500 nm
 61.63 %
@Wavelength 10000 nm
61.63 %
@Wavelength 10000 nm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Schott IRG 24 Infrared Chalcogenide Glass
Schott IRG 26 Infrared Chalcogenide Glass
Schott IRG 25 Infrared Chalcogenide Glass
Schott IRG 22 Infrared Chalcogenide Glass

CSGT9930 / 183183

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.