MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ASTM A387 Alloy Steel, grade 12, Chromium Molybdenum  (discontinued **)
Categories: Metal; Ferrous Metal; ASTM Steel; Tool Steel; Cold Work Steel

Material Notes: 1Cr-0.5Mo STEEL PLATES FOR BOILERS AND PRESSURE VESSELS (SCMV 2 NT)

discontinued in 1989

Creep and rupture data provided by NIMS

Key Words: DIN 17155 13CrMo44; UNS K11757; ISO 2604/IV P32; JIS G4109 SCMV 2 NT
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³Based on UNS number
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 450 - 585 MPa65300 - 84800 psi
Tensile Strength, Yield 275 MPa39900 psi
Elongation at Break 22 %22 %
Rupture Strength  34.0 - 45.0 MPa
@Temperature 575 °C,
Time 3.60e+8 sec
4930 - 6530 psi
@Temperature 1070 °F,
Time 100000 hour
 53.0 - 74.0 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
7690 - 10700 psi
@Temperature 1020 °F,
Time 100000 hour
 79.0 - 104 MPa
@Temperature 525 °C,
Time 3.60e+8 sec
11500 - 15100 psi
@Temperature 977 °F,
Time 100000 hour
 118 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
17100 psi
@Temperature 1110 °F,
Time 100000 hour
 126 - 159 MPa
@Temperature 500 °C,
Time 3.60e+8 sec
18300 - 23100 psi
@Temperature 932 °F,
Time 100000 hour
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.050 - 0.17 %0.050 - 0.17 %
Chromium, Cr 0.80 - 1.15 %0.80 - 1.15 %
Iron, Fe 96.96 - 98.15 %96.96 - 98.15 %
Manganese, Mn 0.40 - 0.65 %0.40 - 0.65 %
Molybdenum, Mo 0.45 - 0.60 %0.45 - 0.60 %
Phosphorus, P <= 0.035 %<= 0.035 %
Silicon, Si 0.15 - 0.40 %0.15 - 0.40 %
Sulfur, S <= 0.035 %<= 0.035 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ASTM A213 T12 Alloy Steel, Chromium Molybdenum
ASTM A213 T22 2.25Cr-1Mo STEEL FOR BOILER AND HEAT EXCHANGER SEAMLESS TUBES (STBA 24)
ASTM A387 Alloy Steel, grade 11, Chromium Molybdenum
ASTM A213 T11 Alloy Steel, Chromium Molybdenum, F11-1
ASTM A387 Alloy Steel, grade 22, Chromium Molybdenum

NIMS008 / 77525

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.