MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ASTM A213 T12 Alloy Steel, Chromium Molybdenum
Categories: Metal; Ferrous Metal; ASTM Steel; Tool Steel; Cold Work Steel

Material Notes: 1Cr-0.5Mo STEEL TUBES FOR BOILERS AND HEAT EXCHANGERS (STBA 22)

Creep and rupture data provided by NIMS

Key Words: DIN 17175 13CrMo44; ISO 2604 II TS32; JIS G3462 STBA 22; UNS K11562
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.75 g/cc0.280 lb/in³Based on UNS number
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 415 MPa60200 psi
Tensile Strength, Yield 220 MPa31900 psi
Elongation at Break 30 %30 %
Rupture Strength  31.0 - 38.0 MPa
@Temperature 575 °C,
Time 3.60e+8 sec
4500 - 5510 psi
@Temperature 1070 °F,
Time 100000 hour
 58.0 - 65.0 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
8410 - 9430 psi
@Temperature 1020 °F,
Time 100000 hour
 86.0 - 96.0 MPa
@Temperature 525 °C,
Time 3.60e+8 sec
12500 - 13900 psi
@Temperature 977 °F,
Time 100000 hour
 127 - 154 MPa
@Temperature 500 °C,
Time 3.60e+8 sec
18400 - 22300 psi
@Temperature 932 °F,
Time 100000 hour
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.050 - 0.15 %0.050 - 0.15 %
Chromium, Cr 0.80 - 1.25 %0.80 - 1.25 %
Iron, Fe 96.79 - 98.41 %96.79 - 98.41 %
Manganese, Mn 0.30 - 0.61 %0.30 - 0.61 %
Molybdenum, Mo 0.44 - 0.65 %0.44 - 0.65 %
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si <= 0.50 %<= 0.50 %
Sulfur, S <= 0.025 %<= 0.025 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ASTM A387 Alloy Steel, grade 12, Chromium Molybdenum
ASTM A213 T22 2.25Cr-1Mo STEEL FOR BOILER AND HEAT EXCHANGER SEAMLESS TUBES (STBA 24)
ASTM A213 T11 Alloy Steel, Chromium Molybdenum, F11-1
ASTM A213 T2 Alloy Steel, Chromium Molybdenum
ASTM A387 Alloy Steel, grade 22, Chromium Molybdenum

NIMS007 / 77524

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.