Physical Properties | Metric | English | Comments |
---|
Density | 8.20 g/cc | 0.296 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Vickers | 175 | 175 |
Tensile Strength, Ultimate | 760 MPa | 110000 psi |
| 100 MPa @Temperature 900 °C | 14500 psi @Temperature 1650 °F |
Tensile Strength, Yield | 390 MPa @Strain 0.2 % | 56600 psi @Strain 0.2 % |
Elongation at Break | 30 % | 30 % |
Creep Strength | 4.00 MPa @Temperature 1000 °C, Time 3.60e+6 sec | 580 psi @Temperature 1830 °F, Time 1000 hour |
| 15.0 MPa @Temperature 800 °C, Time 3.60e+6 sec | 2180 psi @Temperature 1470 °F, Time 1000 hour |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000111 ohm-cm | 0.000111 ohm-cm |
| 0.000113 ohm-cm @Temperature 100 °C | 0.000113 ohm-cm @Temperature 212 °F |
| 0.000115 ohm-cm @Temperature 200 °C | 0.000115 ohm-cm @Temperature 392 °F |
| 0.000116 ohm-cm @Temperature 300 °C | 0.000116 ohm-cm @Temperature 572 °F |
| 0.000117 ohm-cm @Temperature 400 °C | 0.000117 ohm-cm @Temperature 752 °F |
| 0.000120 ohm-cm @Temperature 500 °C | 0.000120 ohm-cm @Temperature 932 °F |
| 0.000121 ohm-cm @Temperature 600 °C | 0.000121 ohm-cm @Temperature 1110 °F |
| 0.000121 ohm-cm @Temperature 700 °C | 0.000121 ohm-cm @Temperature 1290 °F |
| 0.000122 ohm-cm @Temperature 800 °C | 0.000122 ohm-cm @Temperature 1470 °F |
| 0.000122 ohm-cm @Temperature 900 °C | 0.000122 ohm-cm @Temperature 1650 °F |
| 0.000123 ohm-cm @Temperature 1000 °C | 0.000123 ohm-cm @Temperature 1830 °F |
| 0.000124 ohm-cm @Temperature 1100 °C | 0.000124 ohm-cm @Temperature 2010 °F |
| 0.000125 ohm-cm @Temperature 1200 °C | 0.000125 ohm-cm @Temperature 2190 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 14.0 µm/m-°C @Temperature 20.0 - 250 °C | 7.78 µin/in-°F @Temperature 68.0 - 482 °F |
| 15.0 µm/m-°C @Temperature 20.0 - 500 °C | 8.33 µin/in-°F @Temperature 68.0 - 932 °F |
| 16.0 µm/m-°C @Temperature 20.0 - 750 °C | 8.89 µin/in-°F @Temperature 68.0 - 1380 °F |
| 17.0 µm/m-°C @Temperature 20.0 - 1000 °C | 9.44 µin/in-°F @Temperature 68.0 - 1830 °F |
Specific Heat Capacity | 0.460 J/g-°C @Temperature 20.0 °C | 0.110 BTU/lb-°F @Temperature 68.0 °F |
| 0.460 J/g-°C @Temperature 100 °C | 0.110 BTU/lb-°F @Temperature 212 °F |
| 0.480 J/g-°C @Temperature 200 °C | 0.115 BTU/lb-°F @Temperature 392 °F |
| 0.500 J/g-°C @Temperature 300 °C | 0.120 BTU/lb-°F @Temperature 572 °F |
| 0.530 J/g-°C @Temperature 400 °C | 0.127 BTU/lb-°F @Temperature 752 °F |
| 0.550 J/g-°C @Temperature 500 °C | 0.131 BTU/lb-°F @Temperature 932 °F |
| 0.580 J/g-°C @Temperature 600 °C | 0.139 BTU/lb-°F @Temperature 1110 °F |
| 0.600 J/g-°C @Temperature 700 °C | 0.143 BTU/lb-°F @Temperature 1290 °F |
| 0.630 J/g-°C @Temperature 800 °C | 0.151 BTU/lb-°F @Temperature 1470 °F |
| 0.660 J/g-°C @Temperature 900 °C | 0.158 BTU/lb-°F @Temperature 1650 °F |
| 0.680 J/g-°C @Temperature 1000 °C | 0.163 BTU/lb-°F @Temperature 1830 °F |
| 0.710 J/g-°C @Temperature 1100 °C | 0.170 BTU/lb-°F @Temperature 2010 °F |
Thermal Conductivity | 13.0 W/m-K @Temperature 20.0 °C | 90.2 BTU-in/hr-ft²-°F @Temperature 68.0 °F |
| 13.0 W/m-K @Temperature 100 °C | 90.2 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 14.0 W/m-K @Temperature 200 °C | 97.2 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 16.0 W/m-K @Temperature 300 °C | 111 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 17.0 W/m-K @Temperature 400 °C | 118 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 19.0 W/m-K @Temperature 500 °C | 132 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 20.0 W/m-K @Temperature 600 °C | 139 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 22.0 W/m-K @Temperature 700 °C | 153 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 24.0 W/m-K @Temperature 800 °C | 167 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 25.0 W/m-K @Temperature 900 °C | 174 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 25.0 W/m-K @Temperature 1000 °C | 174 BTU-in/hr-ft²-°F @Temperature 1830 °F |
| 29.0 W/m-K @Temperature 1100 °C | 201 BTU-in/hr-ft²-°F @Temperature 2010 °F |
Melting Point | 1390 °C | 2530 °F |
Maximum Service Temperature, Air | 1150 °C | 2100 °F |
|
Optical Properties | Metric | English | Comments |
---|
Emissivity (0-1) | 0.88 | 0.88 |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | <= 0.10 % | <= 0.10 % |
Chromium, Cr | 14 - 18 % | 14 - 18 % |
Iron, Fe | >= 19.2 % | >= 19.2 % |
Manganese, Mn | <= 1.0 % | <= 1.0 % |
Nickel, Ni | 57 - 60 % | 57 - 60 % |
Silicon, Si | 1.0 - 1.7 % | 1.0 - 1.7 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.