MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

Sandvik Nikrothal 60 Resistance Strip
Categories: Metal; Nonferrous Metal; Nickel Alloy

Material Notes: NIKROTHAL 60 is an austenitic NiCrFe alloy which is recommended for use at element temperatures up to 1150°C (2100°F). NIKROTHAL 60 has excellent hot strength, good oxidation properties and very good formability. NIKROTHAL 60 has good corrosion resistance except in sulphur containing atmospheres and certain controlled atmospheres.

Typical applications for NIKROTHAL 60 are as braking resistors and as electrical heating elements in industrial furnaces.

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.20 g/cc0.296 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers  160
@Thickness 4.00 mm
160
@Thickness 0.157 in
 160
@Thickness 76.2 mm
160
@Thickness 3.00 in
 170
@Thickness 1.00 mm
170
@Thickness 0.0394 in
Tensile Strength, Ultimate 100 MPa
@Temperature 900 °C
14500 psi
@Temperature 1650 °F
deformation rate= 6.2x10-2/min
 620 MPa
@Thickness 76.2 mm
89900 psi
@Thickness 3.00 in
 650 MPa
@Thickness 4.00 mm
94300 psi
@Thickness 0.157 in
 700 MPa
@Thickness 1.00 mm
102000 psi
@Thickness 0.0394 in
Tensile Strength, Yield 270 MPa
@Thickness 76.2 mm
39200 psi
@Thickness 3.00 in
 300 MPa
@Strain 0.2 %,
Thickness 4.00 mm
43500 psi
@Strain 0.2 %,
Thickness 0.157 in
 400 MPa
@Strain 0.2 %,
Thickness 1.00 mm
58000 psi
@Strain 0.2 %,
Thickness 0.0394 in
Elongation at Break  35 %
@Thickness 1.00 mm
35 %
@Thickness 0.0394 in
 40 %
@Thickness 4.00 mm
40 %
@Thickness 0.157 in
 40 %
@Thickness 76.2 mm
40 %
@Thickness 3.00 in
Creep Strength  4.00 MPa
@Temperature 1000 °C,
Time 3.60e+6 sec
580 psi
@Temperature 1830 °F,
Time 1000 hour
1% elongation
 15.0 MPa
@Temperature 800 °C,
Time 3.60e+6 sec
2180 psi
@Temperature 1470 °F,
Time 1000 hour
1% elongation
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000111 ohm-cm0.000111 ohm-cm
 0.000113 ohm-cm
@Temperature 100 °C
0.000113 ohm-cm
@Temperature 212 °F
 0.000115 ohm-cm
@Temperature 200 °C
0.000115 ohm-cm
@Temperature 392 °F
 0.000116 ohm-cm
@Temperature 300 °C
0.000116 ohm-cm
@Temperature 572 °F
 0.000117 ohm-cm
@Temperature 400 °C
0.000117 ohm-cm
@Temperature 752 °F
 0.000120 ohm-cm
@Temperature 500 °C
0.000120 ohm-cm
@Temperature 932 °F
 0.000121 ohm-cm
@Temperature 600 °C
0.000121 ohm-cm
@Temperature 1110 °F
 0.000121 ohm-cm
@Temperature 700 °C
0.000121 ohm-cm
@Temperature 1290 °F
 0.000122 ohm-cm
@Temperature 800 °C
0.000122 ohm-cm
@Temperature 1470 °F
 0.000122 ohm-cm
@Temperature 900 °C
0.000122 ohm-cm
@Temperature 1650 °F
 0.000123 ohm-cm
@Temperature 1000 °C
0.000123 ohm-cm
@Temperature 1830 °F
 0.000124 ohm-cm
@Temperature 1100 °C
0.000124 ohm-cm
@Temperature 2010 °F
 0.000125 ohm-cm
@Temperature 1200 °C
0.000125 ohm-cm
@Temperature 2190 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  14.0 µm/m-°C
@Temperature 20.0 - 250 °C
7.78 µin/in-°F
@Temperature 68.0 - 482 °F
 15.0 µm/m-°C
@Temperature 20.0 - 500 °C
8.33 µin/in-°F
@Temperature 68.0 - 932 °F
 16.0 µm/m-°C
@Temperature 20.0 - 750 °C
8.89 µin/in-°F
@Temperature 68.0 - 1380 °F
 17.0 µm/m-°C
@Temperature 20.0 - 1000 °C
9.44 µin/in-°F
@Temperature 68.0 - 1830 °F
Specific Heat Capacity  0.460 J/g-°C
@Temperature 20.0 °C
0.110 BTU/lb-°F
@Temperature 68.0 °F
 0.460 J/g-°C
@Temperature 100 °C
0.110 BTU/lb-°F
@Temperature 212 °F
 0.480 J/g-°C
@Temperature 200 °C
0.115 BTU/lb-°F
@Temperature 392 °F
 0.500 J/g-°C
@Temperature 300 °C
0.120 BTU/lb-°F
@Temperature 572 °F
 0.530 J/g-°C
@Temperature 400 °C
0.127 BTU/lb-°F
@Temperature 752 °F
 0.550 J/g-°C
@Temperature 500 °C
0.131 BTU/lb-°F
@Temperature 932 °F
 0.580 J/g-°C
@Temperature 600 °C
0.139 BTU/lb-°F
@Temperature 1110 °F
 0.600 J/g-°C
@Temperature 700 °C
0.143 BTU/lb-°F
@Temperature 1290 °F
 0.630 J/g-°C
@Temperature 800 °C
0.151 BTU/lb-°F
@Temperature 1470 °F
 0.660 J/g-°C
@Temperature 900 °C
0.158 BTU/lb-°F
@Temperature 1650 °F
 0.680 J/g-°C
@Temperature 1000 °C
0.163 BTU/lb-°F
@Temperature 1830 °F
 0.710 J/g-°C
@Temperature 1100 °C
0.170 BTU/lb-°F
@Temperature 2010 °F
Thermal Conductivity  13.0 W/m-K
@Temperature 20.0 °C
90.2 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 13.0 W/m-K
@Temperature 100 °C
90.2 BTU-in/hr-ft²-°F
@Temperature 212 °F
 14.0 W/m-K
@Temperature 200 °C
97.2 BTU-in/hr-ft²-°F
@Temperature 392 °F
 16.0 W/m-K
@Temperature 300 °C
111 BTU-in/hr-ft²-°F
@Temperature 572 °F
 17.0 W/m-K
@Temperature 400 °C
118 BTU-in/hr-ft²-°F
@Temperature 752 °F
 19.0 W/m-K
@Temperature 500 °C
132 BTU-in/hr-ft²-°F
@Temperature 932 °F
 20.0 W/m-K
@Temperature 600 °C
139 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 22.0 W/m-K
@Temperature 700 °C
153 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 24.0 W/m-K
@Temperature 800 °C
167 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 25.0 W/m-K
@Temperature 900 °C
174 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 25.0 W/m-K
@Temperature 1000 °C
174 BTU-in/hr-ft²-°F
@Temperature 1830 °F
 29.0 W/m-K
@Temperature 1100 °C
201 BTU-in/hr-ft²-°F
@Temperature 2010 °F
Melting Point 1390 °C2530 °F
Maximum Service Temperature, Air 1150 °C2100 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.880.88fully oxidized
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.10 %<= 0.10 %
Chromium, Cr 14 - 18 %14 - 18 %
Iron, Fe >= 19.2 %>= 19.2 %
Manganese, Mn <= 1.0 %<= 1.0 %
Nickel, Ni 57 - 60 %57 - 60 %
Silicon, Si 1.0 - 1.7 %1.0 - 1.7 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Special Metals INCONEL® 625LCF® Nickel Superalloy (UNS N06626) Annealed + 20% Cold Work
Nichrome 60-15 Medium Temperature Resistor Material
Sandvik Nikrothal 40 Resistance Strip
Special Metals INCONEL® 690 Nickel Superalloy, Hot Rolled Flat, 2.0 inch (51 mm) Diameter
Goodfellow Nickel 79/Aluminum 21 Alloy

NSANDV068 / 18962

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.