MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ATI Allvac® Nickelvac® 43-40 UNS G43400, UNS H43400 Specialty Steel  (discontinued **)
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 4000 Series Steel; Low Alloy Steel; Carbon Steel; Low Carbon Steel

Material Notes: Uses: Automotive applications, structural components, gears, rods, heat-treatable shafts.

Property values are for samples in the metallurgical condition: 1550°F quench + 1000°F temper.

Information provided by Allvac, An Allegheny Teledyne Company.

Key Words: AISI 4340; AMS 6359, 6409, 6414, 6415, 6454; ASTM A 29, A 320, A 322, A 331, A 646.
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.83 g/cc0.283 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 5252
Tensile Strength, Ultimate 1964 MPa284900 psi
Tensile Strength, Yield 1861 MPa
@Strain 0.2 %
269900 psi
@Strain 0.2 %
Elongation at Break 10 %10 %
Reduction of Area 38 %38 %
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.40 %0.40 %
Chromium, Cr 0.80 %0.80 %
Iron, Fe 96 %96 %as balance
Manganese, Mn 0.70 %0.70 %
Molybdenum, Mo 0.25 %0.25 %
Nickel, Ni 1.83 %1.83 %
Phosphorus, P 0.020 %0.020 %
Silicon, Si 0.23 %0.23 %
Sulfur, S 0.020 %0.020 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ATI Allvac® Vasco® 4340 Specialty Steel, Heat Treatment: 899°C (1650°F) Q+T
Crucible Steel AISI 4340 Alloy Steel
AISI 4340 Steel, oil quenched 855°C (1570°F), 230°C (450°F) temper for 4 hrs.
AISI 4340 Steel, oil quenched 845°C, 650°C (1200°F) temper
AISI 4340 Steel, oil quenched 800°C (1470°F), 540°C (1000°F) temper, 100 mm (4 in.) round

NALLV27 / 14943

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.