MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Kraton® G1702 H (SEP) Linear Diblock Copolymer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Description: Kraton G1702 H is a clear, linear diblock copolymer based on styrene and ethylene/propylene with a polystyrene content of 28%. It is supplied from North America in the physical form identified:
Kraton G1702 HU - supplied as a powder

Region: Asia Pacific, Europe, Japan, North America, and South America

Uses: Kraton G1702 H is used as an ingredient in formulating adhesives, sealants and coatings. It may also find use as a modifier of bitumen or thermoplastics and in compound formulations.

Applications: Adhesives, Sealant and Coatings; Compounding and Personal Hygiene; Packaging and Polymod; and Personal Care

Information provided by Kraton®

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.910 g/cc0.910 g/ccASTM D4025
Volatiles <= 0.40 %<= 0.40 %KM 04
Kinematic Viscosity at 100°C (212°F) 18 - 22 cSt18 - 22 cSt1.7%, ENJ404; BAM 1201
Melt Flow <= 1.0 g/10 min
@Load 5.00 kg,
Temperature 230 °C
<= 1.0 g/10 min
@Load 11.0 lb,
Temperature 446 °F
 
Chemical PropertiesMetricEnglishComments
Diblock Content 100 %100 %
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 41
@Time 10.0 sec
41
@Time 0.00278 hour
Typical values on polymer compression molded at 350°F; ASTM D2240
Tensile Strength 2.07 MPa300 psiTypical properties of film cast from toluene solution; ASTM D412
Elongation at Break >= 100 %>= 100 %Typical properties of film cast from toluene solution.; ASTM D412
 
Descriptive Properties
ContentNon-staining phenolic antioxidant0.03-0.2%, KM 08
 Polystyrene26.2-29%, Measured on the polymer before hydrogenation, KM 03
Styrene/Rubber Ratio28/72

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Kraton® D1193 P (SIS) Linear Triblock Copolymer
Kraton® FG1901 G (SEBS) grafted with MA
Kraton® A1536 H (SEBS) Linear Triblock Copolymer
Kraton® G1641 H (SEBS) Linear Triblock Copolymer
Kraton® G1651 E (SEBS) Linear Triblock Copolymer

PKRA9904 / 132803

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.