MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Inconel alloy 702, (UNS N07702) Superalloy
Categories: Metal; Nonferrous Metal; Nickel Alloy

Material Notes: Age-hardened

Al3.25-Cr15.5-Fe1-Ni79.5-Ti0.63

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.41 g/cc0.304 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Rupture Strength  16.0 MPa
@Temperature 980 °C,
Time 3.60e+6 sec
2320 psi
@Temperature 1800 °F,
Time 1000 hour
 22.0 MPa
@Temperature 980 °C,
Time 360000 sec
3190 psi
@Temperature 1800 °F,
Time 100 hour
 283 MPa
@Temperature 650 °C,
Time 3.60e+6 sec
41000 psi
@Temperature 1200 °F,
Time 1000 hour
 379 MPa
@Temperature 650 °C,
Time 360000 sec
55000 psi
@Temperature 1200 °F,
Time 100 hour
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 3.25 %3.25 %
Chromium, Cr 15.5 %15.5 %
Iron, Fe 1.0 %1.0 %
Nickel, Ni 79.5 %79.5 %
Titanium, Ti 0.63 %0.63 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Inconel alloy 700, ATG S8 Superalloy
Inconel alloy 722 Superalloy
Special Metals INCONEL® MA758 Oxide-Dispersion-Strengthened Ni-Cr Superalloy
Alloy 713C Cast Nickel Superalloy (UNS N07713)
ATI Allvac® Rene 41® Nickel Superalloy, Heat Treatment: 1079°C (1975°F) + Age

NZ97135 / 200197

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.