MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LyondellBasell Hostalen 4731B High Density Polyethylene (HDPE), Extruded
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Extruded

Material Notes: Hostalen 4731 B is a high density polyethylene (HDPE) with high melt viscosity for extrusion. The product provides excellent stress crack resistance properties (ESCR) combined with very good long term hydrostatic strength, high heat- and extremely high extraction stability. Hostalen 4731 B fulfills the requirements of DIN 16833 / ISO 24033 for PE-RT, Type II. Typical customer applications are under floor heating and multilayer pipes for heating and plumbing. The product is not being sold for use in North America. Applications: Drinking Water Pipe, Plumbing, Heating & Cooling

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.947 g/cc0.0342 lb/in³ISO 1183-1
Oxidative Induction Time (OIT) 40 min
@Temperature 210 °C
40 min
@Temperature 410 °F
ISO 11357-6
Melt Flow  0.45 g/10 min
@Load 5.00 kg,
Temperature 190 °C
0.45 g/10 min
@Load 11.0 lb,
Temperature 374 °F
ISO 1133-1
 9.5 g/10 min
@Load 2.16 kg,
Temperature 190 °C
9.5 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133-1
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 59
@Time 3.00 sec
59
@Time 0.000833 hour
ISO 868
Tensile Strength, Yield 22.0 MPa3190 psi50mm/min; ISO 527-1,-2
Elongation at Break >= 350 %>= 350 %ISO 527-1,-2
Elongation at Yield 8.0 %8.0 %50mm/min; ISO 527-1,-2
Tensile Modulus 0.850 GPa123 ksiISO 527-1,-2
Charpy Impact, Notched  0.800 J/cm²
@Temperature -30.0 °C
3.81 ft-lb/in²
@Temperature -22.0 °F
ISO 179-1/1eA
 2.40 J/cm²
@Temperature 23.0 °C
11.4 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1/1eA
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 70.0 °C158 °FB50; ISO 306
 120 °C248 °FA50; ISO 306
 
Descriptive Properties
MRS Classification (MPA)10ISO 9080
Processing MethodPipe, sheet

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Hostalen 4131B High Density Polyethylene (HDPE), Extruded
Iran Petrochemical (PCC) EX 6HT HM 9455 HT High Density Polyethylene
LyondellBasell Hostalen CRP 100 RT BLACK High Density Polyethylene (HDPE), Pipe Grade
Ineos TUB 121N HDPE
Ineos TUB 121 HDPE

PEQT8443 / 220078

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.