Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 4.04 g/cc | 4.04 g/cc |
|
Chemical Properties | Metric | English | Comments |
---|
Acid Class, SR | 51 | 51 |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 720 @Load 0.0999 kg | 720 @Load 0.220 lb |
Modulus of Elasticity | 119.0 GPa | 17260 ksi |
Modulus of Rigidity | 46.1 GPa | 6690 ksi |
Poissons Ratio | 0.291 | 0.291 |
Abrasion | 65 | 65 |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 5.70 µm/m-°C @Temperature -30.0 - 70.0 °C | 3.17 µin/in-°F @Temperature -22.0 - 158 °F |
| 7.00 µm/m-°C @Temperature 100 - 300 °C | 3.89 µin/in-°F @Temperature 212 - 572 °F |
Thermal Conductivity | 0.861 W/m-K @Temperature 35.0 °C | 5.98 BTU-in/hr-ft²-°F @Temperature 95.0 °F |
Transformation Temperature, Tg | 653 °C | 1210 °F |
Softening Point | 724 °C | 1340 °F |
Annealing Point | 646 °C | 1190 °F |
Strain Point | 631 °C | 1170 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.70016 @Wavelength 2325.42 nm | 1.70016 @Wavelength 2325.42 nm |
| 1.70787 @Wavelength 1970.09 nm | 1.70787 @Wavelength 1970.09 nm |
| 1.71598 @Wavelength 1529.58 nm | 1.71598 @Wavelength 1529.58 nm |
| 1.72297 @Wavelength 1128.64 nm | 1.72297 @Wavelength 1128.64 nm |
| 1.72525 @Wavelength 1013.98 nm | 1.72525 @Wavelength 1013.98 nm |
| 1.72918 @Wavelength 852.11 nm | 1.72918 @Wavelength 852.11 nm |
| 1.73186 @Wavelength 768.19 nm | 1.73186 @Wavelength 768.19 nm |
| 1.73430 @Wavelength 706.52 nm | 1.73430 @Wavelength 706.52 nm |
| 1.73673 @Wavelength 656.27 nm | 1.73673 @Wavelength 656.27 nm |
| 1.73741 @Wavelength 643.85 nm | 1.73741 @Wavelength 643.85 nm |
| 1.73804 @Wavelength 632.8 nm | 1.73804 @Wavelength 632.8 nm |
| 1.74087 @Wavelength 589.29 nm | 1.74087 @Wavelength 589.29 nm |
| 1.74100 @Wavelength 587.56 nm | 1.74100 @Wavelength 587.56 nm |
| 1.74435 @Wavelength 546.07 nm | 1.74435 @Wavelength 546.07 nm |
| 1.75080 @Wavelength 486.13 nm | 1.75080 @Wavelength 486.13 nm |
| 1.75161 @Wavelength 479.99 nm | 1.75161 @Wavelength 479.99 nm |
| 1.75748 @Wavelength 441.57 nm | 1.75748 @Wavelength 441.57 nm |
| 1.75850 @Wavelength 435.835 nm | 1.75850 @Wavelength 435.835 nm |
| 1.76491 @Wavelength 404.656 nm | 1.76491 @Wavelength 404.656 nm |
| 1.77589 @Wavelength 365.015 nm | 1.77589 @Wavelength 365.015 nm |
Abbe Number | 52.41 | 52.41 |
| 52.64 | 52.64 |
Optical Dispersion | 0.004272 | 0.004272 |
| 0.004871 | 0.004871 |
| 0.006413 | 0.006413 |
| 0.006948 | 0.006948 |
| 0.007255 | 0.007255 |
| 0.007627 | 0.007627 |
| 0.007696 | 0.007696 |
| 0.011481 | 0.011481 |
| 0.01216 | 0.01216 |
| 0.014078 | 0.014078 |
| 0.014203 | 0.014203 |
| 0.017393 | 0.017393 |
| 0.017502 | 0.017502 |
| 0.024285 | 0.024285 |
Transmission, Visible | 93.5 % @Wavelength 380 nm | 93.5 % @Wavelength 380 nm |
| 95.8 % @Wavelength 390 nm | 95.8 % @Wavelength 390 nm |
| 97.1 % @Wavelength 400 nm | 97.1 % @Wavelength 400 nm |
| 98.2 % @Wavelength 420 nm | 98.2 % @Wavelength 420 nm |
| 98.8 % @Wavelength 440 nm | 98.8 % @Wavelength 440 nm |
| 99.1 % @Wavelength 460 nm | 99.1 % @Wavelength 460 nm |
| 99.4 % @Wavelength 480 nm | 99.4 % @Wavelength 480 nm |
| 99.6 % @Wavelength 500 nm | 99.6 % @Wavelength 500 nm |
| 99.7 % @Wavelength 550 nm | 99.7 % @Wavelength 550 nm |
| 99.7 % @Wavelength 600 nm | 99.7 % @Wavelength 600 nm |
| 99.7 % @Wavelength 650 nm | 99.7 % @Wavelength 650 nm |
| 99.8 % @Wavelength 700 nm | 99.8 % @Wavelength 700 nm |
IR Transmittance | 62 % @Wavelength 2400 nm | 62 % @Wavelength 2400 nm |
| 88 % @Wavelength 2200 nm | 88 % @Wavelength 2200 nm |
| 98.5 % @Wavelength 1800 nm | 98.5 % @Wavelength 1800 nm |
| 99.4 % @Wavelength 1400 nm | 99.4 % @Wavelength 1400 nm |
| 99.4 % @Wavelength 1600 nm | 99.4 % @Wavelength 1600 nm |
| 99.8 % @Wavelength 800 nm | 99.8 % @Wavelength 800 nm |
| 99.8 % @Wavelength 900 nm | 99.8 % @Wavelength 900 nm |
| 99.8 % @Wavelength 1000 nm | 99.8 % @Wavelength 1000 nm |
| 99.8 % @Wavelength 1200 nm | 99.8 % @Wavelength 1200 nm |
UV Transmittance | 2.0 % @Wavelength 290 nm | 2.0 % @Wavelength 290 nm |
| 7.0 % @Wavelength 300 nm | 7.0 % @Wavelength 300 nm |
| 15 % @Wavelength 310 nm | 15 % @Wavelength 310 nm |
| 27 % @Wavelength 320 nm | 27 % @Wavelength 320 nm |
| 43 % @Wavelength 330 nm | 43 % @Wavelength 330 nm |
| 59 % @Wavelength 340 nm | 59 % @Wavelength 340 nm |
| 72 % @Wavelength 350 nm | 72 % @Wavelength 350 nm |
| 82 % @Wavelength 360 nm | 82 % @Wavelength 360 nm |
| 89 % @Wavelength 370 nm | 89 % @Wavelength 370 nm |
|
Descriptive Properties |
---|
Acid Resistance, Powder Method, RAP) | 4 |
CCI | 0.00 B |
| 0.58 G |
| 0.58 R |
coloring, λ 5 | 280 |
coloring, λ 80 | 365 |
Coloring, Internal Transmission λ 0.05 | 296 |
Coloring, Internal Transmission λ 0.80 | 358 |
Knoop Hardness Class | 7 |
Melt Frequency | 2 |
Ohara Code d | 741527 |
Ohara Code e | 744524 |
Ohara Status | Preferred |
Phosphate Resistance, PR | 2 |
Photoelastic Constant (ß) | 1.55 |
Relative Price | 8 |
Water Resistance, RW(P) | 1 |
Weathering Resistance (Surface Method) W(S)max | 1 |
Weathering Resistance (Surface Method) W(S)min | 2 |
Yield Point, At (°C) | 688 |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.