Physical Properties | Metric | English | Comments |
---|
Density | 3.55 g/cc | 0.128 lb/in³ |
|
Chemical Properties | Metric | English | Comments |
---|
Acid Class, SR | 2.2 | 2.2 |
Alkali Class, AR | 1.0 | 1.0 |
Stain Resistance Class, FR | 0.00 | 0.00 |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 550 | 550 |
Modulus of Elasticity | 78.0 GPa | 11300 ksi |
Poissons Ratio | 0.263 | 0.263 |
Shear Modulus | 30.9 GPa | 4480 ksi |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 6.00 µm/m-°C @Temperature -30.0 - 70.0 °C | 3.33 µin/in-°F @Temperature -22.0 - 158 °F |
| 7.10 µm/m-°C @Temperature 20.0 - 300 °C | 3.94 µin/in-°F @Temperature 68.0 - 572 °F |
Specific Heat Capacity | 0.595 J/g-°C | 0.142 BTU/lb-°F |
Thermal Conductivity | 0.776 W/m-K | 5.39 BTU-in/hr-ft²-°F |
Transformation Temperature, Tg | 659 °C | 1220 °F |
Softening Point | 823 °C | 1510 °F |
Annealing Point | 659 °C | 1220 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.578 @Wavelength 2323.4 nm | 1.578 @Wavelength 2323.4 nm |
| 1.583 @Wavelength 1970.1 nm | 1.583 @Wavelength 1970.1 nm |
| 1.589 @Wavelength 1529.6 nm | 1.589 @Wavelength 1529.6 nm |
| 1.594 @Wavelength 1060 nm | 1.594 @Wavelength 1060 nm |
| 1.595 @Wavelength 1014 nm | 1.595 @Wavelength 1014 nm |
| 1.598 @Wavelength 852.1 nm | 1.598 @Wavelength 852.1 nm |
| 1.602 @Wavelength 706.5 nm | 1.602 @Wavelength 706.5 nm |
| 1.604 @Wavelength 643.8 nm | 1.604 @Wavelength 643.8 nm |
| 1.604 @Wavelength 656.3 nm | 1.604 @Wavelength 656.3 nm |
| 1.605 @Wavelength 632.8 nm | 1.605 @Wavelength 632.8 nm |
| 1.607 @Wavelength 587.6 nm | 1.607 @Wavelength 587.6 nm |
| 1.607 @Wavelength 589.3 nm | 1.607 @Wavelength 589.3 nm |
| 1.609 @Wavelength 546.1 nm | 1.609 @Wavelength 546.1 nm |
| 1.614 @Wavelength 486.1 nm | 1.614 @Wavelength 486.1 nm |
| 1.615 @Wavelength 480 nm | 1.615 @Wavelength 480 nm |
| 1.62 @Wavelength 435.8 nm | 1.62 @Wavelength 435.8 nm |
| 1.625 @Wavelength 404.7 nm | 1.625 @Wavelength 404.7 nm |
| 1.633 @Wavelength 365 nm | 1.633 @Wavelength 365 nm |
| 1.643 @Wavelength 334.1 nm | 1.643 @Wavelength 334.1 nm |
Abbe Number | 56.37 | 56.37 |
| 56.65 | 56.65 |
Optical Dispersion | 0.010722 | 0.010722 |
| 0.010821 | 0.010821 |
Transmission, Visible | 99.1 % @Thickness 25.0 mm, Wavelength 436 nm | 99.1 % @Thickness 0.984 in, Wavelength 436 nm |
| 99.2 % @Thickness 25.0 mm, Wavelength 460 nm | 99.2 % @Thickness 0.984 in, Wavelength 460 nm |
| 99.2 % @Thickness 25.0 mm, Wavelength 420 nm | 99.2 % @Thickness 0.984 in, Wavelength 420 nm |
| 99.5 % @Thickness 25.0 mm, Wavelength 500 nm | 99.5 % @Thickness 0.984 in, Wavelength 500 nm |
| 99.6 % @Thickness 25.0 mm, Wavelength 660 nm | 99.6 % @Thickness 0.984 in, Wavelength 660 nm |
| 99.6 % @Thickness 25.0 mm, Wavelength 620 nm | 99.6 % @Thickness 0.984 in, Wavelength 620 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 436 nm | 99.6 % @Thickness 0.394 in, Wavelength 436 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 460 nm | 99.7 % @Thickness 0.394 in, Wavelength 460 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 420 nm | 99.7 % @Thickness 0.394 in, Wavelength 420 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 700 nm | 99.7 % @Thickness 0.984 in, Wavelength 700 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 546 nm | 99.7 % @Thickness 0.984 in, Wavelength 546 nm |
| 99.7 % @Thickness 25.0 mm, Wavelength 580 nm | 99.7 % @Thickness 0.984 in, Wavelength 580 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 500 nm | 99.8 % @Thickness 0.394 in, Wavelength 500 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 660 nm | 99.8 % @Thickness 0.394 in, Wavelength 660 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 620 nm | 99.8 % @Thickness 0.394 in, Wavelength 620 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 700 nm | 99.9 % @Thickness 0.394 in, Wavelength 700 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 546 nm | 99.9 % @Thickness 0.394 in, Wavelength 546 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 580 nm | 99.9 % @Thickness 0.394 in, Wavelength 580 nm |
IR Transmittance | 58.5 % @Thickness 25.0 mm, Wavelength 2500 nm | 58.5 % @Thickness 0.984 in, Wavelength 2500 nm |
| 74.8 % @Thickness 25.0 mm, Wavelength 2325 nm | 74.8 % @Thickness 0.984 in, Wavelength 2325 nm |
| 80.7 % @Thickness 10.0 mm, Wavelength 2500 nm | 80.7 % @Thickness 0.394 in, Wavelength 2500 nm |
| 89 % @Thickness 10.0 mm, Wavelength 2325 nm | 89 % @Thickness 0.394 in, Wavelength 2325 nm |
| 93 % @Thickness 25.0 mm, Wavelength 1970 nm | 93 % @Thickness 0.984 in, Wavelength 1970 nm |
| 97.1 % @Thickness 10.0 mm, Wavelength 1970 nm | 97.1 % @Thickness 0.394 in, Wavelength 1970 nm |
| 98.7 % @Thickness 25.0 mm, Wavelength 1530 nm | 98.7 % @Thickness 0.984 in, Wavelength 1530 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 1530 nm | 99.5 % @Thickness 0.394 in, Wavelength 1530 nm |
| 99.6 % @Thickness 25.0 mm, Wavelength 1060 nm | 99.6 % @Thickness 0.984 in, Wavelength 1060 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 1060 nm | 99.8 % @Thickness 0.394 in, Wavelength 1060 nm |
UV Transmittance | 1.0 % @Thickness 10.0 mm, Wavelength 290 nm | 1.0 % @Thickness 0.394 in, Wavelength 290 nm |
| 9.2 % @Thickness 25.0 mm, Wavelength 310 nm | 9.2 % @Thickness 0.984 in, Wavelength 310 nm |
| 13 % @Thickness 10.0 mm, Wavelength 300 nm | 13 % @Thickness 0.394 in, Wavelength 300 nm |
| 34.6 % @Thickness 25.0 mm, Wavelength 320 nm | 34.6 % @Thickness 0.984 in, Wavelength 320 nm |
| 38.5 % @Thickness 10.0 mm, Wavelength 310 nm | 38.5 % @Thickness 0.394 in, Wavelength 310 nm |
| 65.4 % @Thickness 10.0 mm, Wavelength 320 nm | 65.4 % @Thickness 0.394 in, Wavelength 320 nm |
| 70.3 % @Thickness 25.0 mm, Wavelength 334 nm | 70.3 % @Thickness 0.984 in, Wavelength 334 nm |
| 86.9 % @Thickness 10.0 mm, Wavelength 334 nm | 86.9 % @Thickness 0.394 in, Wavelength 334 nm |
| 89.2 % @Thickness 25.0 mm, Wavelength 350 nm | 89.2 % @Thickness 0.984 in, Wavelength 350 nm |
| 95.5 % @Thickness 10.0 mm, Wavelength 350 nm | 95.5 % @Thickness 0.394 in, Wavelength 350 nm |
| 95.7 % @Thickness 25.0 mm, Wavelength 365 nm | 95.7 % @Thickness 0.984 in, Wavelength 365 nm |
| 96.8 % @Thickness 25.0 mm, Wavelength 370 nm | 96.8 % @Thickness 0.984 in, Wavelength 370 nm |
| 98 % @Thickness 25.0 mm, Wavelength 380 nm | 98 % @Thickness 0.984 in, Wavelength 380 nm |
| 98.3 % @Thickness 10.0 mm, Wavelength 365 nm | 98.3 % @Thickness 0.394 in, Wavelength 365 nm |
| 98.6 % @Thickness 25.0 mm, Wavelength 390 nm | 98.6 % @Thickness 0.984 in, Wavelength 390 nm |
| 98.7 % @Thickness 10.0 mm, Wavelength 370 nm | 98.7 % @Thickness 0.394 in, Wavelength 370 nm |
| 99 % @Thickness 25.0 mm, Wavelength 400 nm | 99 % @Thickness 0.984 in, Wavelength 400 nm |
| 99.1 % @Thickness 25.0 mm, Wavelength 405 nm | 99.1 % @Thickness 0.984 in, Wavelength 405 nm |
| 99.2 % @Thickness 10.0 mm, Wavelength 380 nm | 99.2 % @Thickness 0.394 in, Wavelength 380 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 390 nm | 99.4 % @Thickness 0.394 in, Wavelength 390 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 400 nm | 99.6 % @Thickness 0.394 in, Wavelength 400 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 405 nm | 99.6 % @Thickness 0.394 in, Wavelength 405 nm |
|
Descriptive Properties |
---|
Climatic resistance | 2 |
Phosphate resistance | 2.3 |
Stress optical coefficient | 2.31 |