MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI adhesives

Multibase C6-135 Dow-Corning Class VI Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes:

Information provided by Multibase

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 3636no post cure; ASTM D2240
 5050post cured- 2 hours at 177°C; ASTM D2240
 5050post cured- 4 hours at 177°C; ASTM D2240
 5050post cured- 8 hours at 177°C; ASTM D2240
Tensile Strength, Ultimate 8.198 MPa1189 psipost cured- 4 hours at 177°C; ASTM D412
 8.281 MPa1201 psino post cure; ASTM D412
 8.749 MPa1269 psipost cured- 2 hours at 177°C; ASTM D412
 8.936 MPa1296 psipost cured- 8 hours at 177°C; ASTM D412
Tensile Strength, Yield 1.23 MPa178 psiat 200%, no post cure; ASTM D412
 2.10 MPa304 psiat 200%, post cured- 2 hours at 177°C; ASTM D412
 2.11 MPa306 psi200%, post cured- 4 hours at 177°C; ASTM D412
 2.14 MPa310 psi200%, post cured- 8 hours at 177°C; ASTM D412
Elongation at Break 814 %814 %post cured- 4 hours at 177°C; ASTM D412
 843 %843 %post cured- 8 hours at 177°C; ASTM D412
 847 %847 %post cured- 2 hours at 177°C; ASTM D412
 1117 %1117 %no post cure; ASTM D412
Tear Strength 35.2 kN/m201 pliDie B, no post cure; ASTM D624
 35.9 kN/m205 pliDie B, post cured- 4 hours at 177°C; ASTM D624
 36.3 kN/m207 pliDie B, post cured- 8 hours at 177°C; ASTM D624
 37.9 kN/m216 pliDie B, post cured- 2 hours at 177°C; ASTM D624
 
Thermal PropertiesMetricEnglishComments
Shrinkage 2.4 %2.4 %no post cure
 2.9 %
@Temperature 177 °C,
Time 7200 sec
2.9 %
@Temperature 351 °F,
Time 2.00 hour
post cured
 3.0 %
@Temperature 177 °C,
Time 14400 sec
3.0 %
@Temperature 351 °F,
Time 4.00 hour
post cured
 3.0 %
@Temperature 177 °C,
Time 28800 sec
3.0 %
@Temperature 351 °F,
Time 8.00 hour
post cured
 
Compliance PropertiesMetricEnglishComments
USP Class VI YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow C6-135 ELASTOMER KIT
Dow C6-150 ELASTOMER KIT
Wacker Elastosil® R plus 4000/50 Silicone Rubber
Dow Silastic® Q7-4750 BIOMEDICAL GRADE ETR ELASTOMER, KIT
CPT C-Flex® R70-190 Opaque Biocompatible TPE

PMULTI165 / 54069

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.