Celanese Zytel® 73G50HSLA BK416 PA6-GF50
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, 50% Glass Fiber Filled
Material Notes:
50% Glass Reinforced, Heat Stabilized, Polyamide 6
Former DuPont product acquired by Celanese in 2022.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.58
g/cc
0.0571
lb/in³
DAM; ISO 1183
Melt Density
1.24
g/cc
@Temperature 270 °C
0.0448
lb/in³
@Temperature 518 °F
Water Absorption
4.5 %
@Thickness 2.00 mm
4.5 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Moisture Absorption
1.60 %
@Thickness 2.00 mm
1.60 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Linear Mold Shrinkage, Flow
0.0010
cm/cm
0.0010
in/in
DAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse
0.0070
cm/cm
0.0070
in/in
DAM; ISO 294-4, 2577
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
150
MPa
21800
psi
50% RH; ISO 527-1/-2
230
MPa
33400
psi
DAM; ISO 527-1/-2
Elongation at Break
2.2 %
2.2 %
DAM; ISO 527-1/-2
4.0 %
4.0 %
50% RH; ISO 527-1/-2
Tensile Modulus
12.0
GPa
1740
ksi
50% RH; ISO 527-1/-2
16.0
GPa
2320
ksi
DAM; ISO 527-1/-2
Flexural Strength
240
MPa
34800
psi
50% RH; ISO 178
400
MPa
58000
psi
DAM; ISO 178
225
MPa
@Strain 3.5 %
32600
psi
@Strain 3.5 %
50% RH; ISO 178
Flexural Modulus
10.0
GPa
1450
ksi
50% RH; ISO 178
15.0
GPa
2180
ksi
DAM; ISO 178
Poissons Ratio
0.33
0.33
50% RH
0.33
0.33
DAM
Charpy Impact Unnotched
9.00
J/cm²
@Temperature -30.0 °C
42.8
ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eU
10.0
J/cm²
@Temperature -30.0 °C
47.6
ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eU
10.0
J/cm²
@Temperature 23.0 °C
47.6
ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eU
10.0
J/cm²
@Temperature 23.0 °C
47.6
ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
Charpy Impact, Notched
1.80
J/cm²
@Temperature -30.0 °C
8.57
ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eA
1.90
J/cm²
@Temperature -30.0 °C
9.04
ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
2.10
J/cm²
@Temperature 23.0 °C
9.99
ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
2.20
J/cm²
@Temperature 23.0 °C
10.5
ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eA
Tensile Creep Modulus, 1 hour
9500
MPa
1.38e+6
psi
1h; 50% RH; ISO 899-1
Tensile Creep Modulus, 1000 hours
7500
MPa
1.09e+6
psi
1000h; 50% RH; ISO 899-1
Electrical Properties
Metric
English
Comments
Surface Resistance
5.00e+12
ohm
5.00e+12
ohm
50% RH; IEC 62631-3-2
Comparative Tracking Index
380
V
380
V
DAM; IEC 60112
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
15.0
µm/m-°C
8.33
µin/in-°F
DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow
100
µm/m-°C
55.6
µin/in-°F
DAM; ISO 11359-1/-2
Specific Heat Capacity
2.05
J/g-°C
@Temperature 270 °C
0.490
BTU/lb-°F
@Temperature 518 °F
Melt
Thermal Conductivity
0.260
W/m-K
@Temperature 270 °C
1.80
BTU-in/hr-ft²-°F
@Temperature 518 °F
Melt
Melting Point
219
°C
426
°F
10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi)
219
°C
426
°F
DAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi)
212
°C
414
°F
DAM; ISO 75-1/-2
Vicat Softening Point
215
°C
419
°F
50°C/h, 50N; DAM; ISO 306
Glass Transition Temp, Tg
15.0
°C
59.0
°F
10°C/min; 50% RH; ISO 11357-1/-2
60.0
°C
140
°F
10°C/min; DAM; ISO 11357-1/-2
Flammability, UL94
HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
DAM; IEC 60695-11-10
Flame Spread
31.0
mm/min
@Thickness 1.00 mm
1.22
in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
Processing Properties
Metric
English
Comments
Melt Temperature
270
°C
518
°F
Optimum, Injection
260
-
280
°C
500
-
536
°F
Range, Injection
Mold Temperature
70.0
-
120
°C
158
-
248
°F
Injection
100
°C
212
°F
Optimum, Injection
Drying Temperature
80.0
°C
176
°F
Injection
Dry Time
2.00
-
4.00
hour
2.00
-
4.00
hour
Injection, Dehumidified Dryer
Moisture Content
<= 0.20 %
<= 0.20 %
Injection
Hold Pressure
50.0
-
100
MPa
7250
-
14500
psi
Range, Injection
Descriptive Properties
Additives
Release agent
Drying Recommended
yes
Injection
FMVSS Class
B
ISO 3795 (FMVSS 302)
ISO designation
ISO 16396-PA6,GF50,M1CGHR,S09-160
Max. screw tangential speed (m/s)
0.2
Injection
Part Marking Code
>PA6-GF50<
ISO 11469
Polymer
PA6-GF50
Processing Hold Pressure Time (s/mm)
3
Injection
Resin Identification
PA6-GF50
ISO 1043
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Asahi Kasei Thermylon® NSG-240A 50% Ceramic and Glass Fiber Reinforced Nylon 6
EMS-Grivory Grilon® BG-50 PA6-GF50
Celanese Zytel® 70G50HSLA BK039B PA66-GF50
Celanese Zytel® 73G35HSL BK262 PA6-GF35
Celanese Zytel® 73G15HSL BK363 PA6-GF15
PDSX5363 / 198003
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.