MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

DuPont™ Kapton® 300HN Polyimide Film, 75 Micron Thickness
Categories: Polymer; Film; Thermoset; Polyimide, TS; Polyimide, Thermoset Film

Material Notes: Film thickness 75 micron (3.0 mil)

All purpose polyimide film. Can be laminated, diecut, slit, formed, or adhesive-coated. Available in thicknesses from 0.3 mil (7.5 µm) to 5 mil (125 µm).

General Kapton® information: Kapton® is synthesized by polymerizing an aromatic dianhydride with an aromatic diamine. It has excellent chemical resistance; there are no known organic solvents for the film. It does not melt. It can be used at both high and low temperature extremes. Kapton® polyimide films can be used in a variety of electrical and electronic uses: wire and cable tapes, formed coil insulation, substrates for printed circuit boards, motor slot liners, magnet wire insulation, transformer and capacitor insulation, magnetic and pressure-sensitive tapes, and tubing.

Data provided by DuPont High Performance Films.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.42 g/cc0.0513 lb/in³
Water Absorption 2.8 %2.8 %24 hr/23°C. ASTM D570
Moisture Absorption at Equilibrium 1.8 %1.8 %50% RH; 23°C
Water Vapor Transmission 3.50 g/m²/day0.225 g/100 in²/day25 µm film; ASTM E-96-92
Oxygen Transmission 9.90 cc-mm/m²-24hr-atm25.1 cc-mil/100 in²-24hr-atm25 µm film; ASTM D1434-82; 50% RH
Thickness 1910 microns75.0 mil
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 69.0 MPa10000 psi25 µm film; 3% yield point, orientation not specified; ASTM D882-91
Film Elongation at Break, MD 75 %75 %Orientation not specified; ASTM D882
Poissons Ratio 0.340.34Avg. three samples elongated at 5%, 7%, 10%
Secant Modulus 2.80 GPa406 ksiASTM D882
Impact Test 0.780 J
@Thickness 0.0250 mm
0.575 ft-lb
@Thickness 0.000984 in
film; Impact strength per DuPont Pneumatic Impact Test
Coefficient of Friction, Dynamic 0.480.48film to film; ASTM D1894-90
Coefficient of Friction, Static 0.630.63film to film; ASTM D1894-90
Film Tensile Strength at Break, MD 221 MPa32100 psiOrientation not specified; ASTM D882
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+10 ohm-cm1.00e+10 ohm-cmin damp heat; IPC-TM-650; Method 2.5.17
 1.40e+17 ohm-cm1.40e+17 ohm-cmper ASTM D257-91
Dielectric Constant  3.5
@Frequency 100000 Hz
3.5
@Frequency 100000 Hz
 3.6
@Frequency 1000 Hz
3.6
@Frequency 1000 Hz
Use evaporated metal electrodes, two terminal system of measurement at standard conditions.; ASTM D150
Dielectric Strength 197 kV/mm5000 kV/inFlat sheets in air; 1/4 in diameter brass electrodes with 0.8 mm edge radius; 60 cps AC at 600V/s; ASTM D149-81
Dissipation Factor  0.0020
@Frequency 1000 Hz
0.0020
@Frequency 1000 Hz
 0.0090
@Frequency 100000 Hz
0.0090
@Frequency 100000 Hz
 
Thermal PropertiesMetricEnglishComments
CTE, linear  20.0 µm/m-°C
@Temperature -14.0 - 38.0 °C
11.1 µin/in-°F
@Temperature 6.80 - 100 °F
25 µm film; ASTM D696-91
 32.0 µm/m-°C
@Temperature 100 - 200 °C
17.8 µin/in-°F
@Temperature 212 - 392 °F
25 µm film
 40.0 µm/m-°C
@Temperature 200 - 300 °C
22.2 µin/in-°F
@Temperature 392 - 572 °F
25 µm film
Specific Heat Capacity 1.09 J/g-°C0.261 BTU/lb-°FDifferential Calorimetry
Thermal Conductivity 0.120 W/m-K0.833 BTU-in/hr-ft²-°FASTM F433-77
Maximum Service Temperature, Air 400 °C752 °FKapton® can function after brief exposure to 400°C (750°F). Various grades are UL rated for continuous service at 220-240°C (430-460°F).
Minimum Service Temperature, Air -269 °C-452 °FMaintains properties and flexibility
Glass Transition Temp, Tg 360 - 410 °C680 - 770 °FA 2nd order transition occurs in Kapton® between 360-410°C (680-770°F) and is assumed to be the Tg
Flammability, UL94 V-0V-0
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.70
@Wavelength 589.3 nm
1.70
@Wavelength 589.3 nm
Na D line; ASTM D542-90

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Teijin Films Teonex® Q51 Polyester Film, 48 Gauge
DuPont Teijin Films Teonex® Q83 Polyester Film, 200 Gauge
DuPont™ Kapton® 300ZT Polyimide Film, 75 Micron Thickness
DuPont™ Nomex® 410 Paper, 3 mil Nominal Thickness
DuPont™ Kapton® 300KN Polyimide Film, 75 Micron Thickness

PDUK03 / 33373

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.